Metallic PBT (Polybutylene Terephthalate) composite material as well as preparation equipment and preparation method thereof

By using a combination of surface-coated metallic pigments and a twin-screw extruder, the problem of easy oxidation or crushing of metallic pigments at high temperatures was solved, and a high-temperature resistant PBT composite material with good metallic texture was prepared, achieving a balance between high performance and aesthetics.

CN118931125AInactive Publication Date: 2024-11-12FOSHAN XINSU NEW MATERIAL TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411170668.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing technologies struggle to produce paint-free engineering plastics that are heat-resistant, have a good metallic texture, and are close to the hardness of metals. Furthermore, metallic pigments are easily oxidized or crushed during the preparation process, resulting in a poor appearance.

Method used

Metallic PBT composite materials were prepared by using surface-coated metallic pigments and a twin-screw extruder, with the metallic pigments protected by shearing kneading blocks and conveying plasticizing threads, combined with specific resins and toughening agents.

Benefits of technology

The resulting PBT composite material is brightly colored, heat-resistant, and has a pearlescent and metallic sheen. It is stable in performance, low in cost, and suitable for long-term production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931125A_ABST
    Figure CN118931125A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of composite materials, and particularly relates to a metal-texture PBT composite material and preparation equipment and a preparation method thereof.The preparation method comprises the steps that PBT resin, PET resin, a flexibilizer, an anti-floating fiber agent, glass fiber powder, surface coating layer metal pigment, a nucleating agent, a hindered phenol antioxidant, a phosphate antioxidant and the like are evenly mixed according to the formula proportion; the PBT composite material which is bright in color, has pearly luster and metal texture, is high-temperature-resistant and high-strength can be prepared by adding the components in a corresponding sequence by using a double-screw extruder with special screw elements and permutation and combination design, and has remarkable substantive features.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of composite materials, and in particular to a metallic-texture PBT composite material and a preparation device and a preparation method thereof. Background Art

[0002] As the international environmental protection situation becomes increasingly demanding, spray-painted plastic products are becoming less and less popular, and spray-free engineering plastics with pearlescent luster and metallic texture have become the new favorite of the times. Many material companies have invested considerable manpower, material and financial resources in the development of spray-free engineering plastics, and have also achieved certain results, mainly PE or PP general-purpose plastics with low processing temperature and imitation metal appearance. They are soft in texture, low in temperature resistance, and have no metallic texture. They are mainly extruded or injection molded into daily chemical packaging materials, air conditioner shells, refrigerator shells, etc.

[0003] However, there is almost no spray-free engineering plastics that are resistant to high temperatures and have a texture close to that of metal hardness, and they are extremely rare in market applications. The main reason is that metal pigments such as aluminum powder, copper-zinc powder, and pearlescent powder with a metallic look have low temperature resistance and are easily oxidized and grayed under high temperature conditions. It is these metal pigments that can bring a shiny effect because of their flake structure, but they are easily squeezed and crushed by the screw during processing and become dull, thus losing their metallic texture. Since metal pigments have extremely poor compatibility with plastics, flow marks are easily formed during the injection molding process, further limiting the practical application of engineering plastics with a metallic texture.

[0004] For example, the patent document with patent number CN201410361318.2 and titled "Spray-free Imitation Metallic PBT and Preparation Method Thereof" discloses a method for preparing spray-free Imitation Metallic PBT, which uses a screw extruder with a screw length-to-diameter ratio of 44:1 and at least two side feeding ports, and adds PBT resin, EBA toughening agent, dispersant and 1 / 3 of metal powder from the main feeding port, and adds glass fiber from the glass fiber feeding port. The remaining dispersant is divided into equal parts and added from two side feeding ports respectively to make spray-free Imitation Metallic PBT particles. Although this solution directly adds metal powder to the PBT resin; uses a composite dispersant mixed with barium stearate, cadmium stearate, and ethylene bisstearamide, and then increases the aspect ratio of the screw extruder granulator, and uses double side feeding to add the metal powder from three different places, so that it is evenly dispersed to avoid agglomeration. At the same time, the addition of toughening agent ensures the tensile and impact properties. The resulting spray-free imitation metal PBT has uniform color and stable performance, but it cannot solve the problem that the metal powder is easily heated and crushed in the extruder, resulting in a poor appearance. Summary of the invention

[0005] In order to solve the problem that there is a lack of solutions on the market for producing spray-free engineering plastics with good metallic texture, high temperature resistance and close to the hardness of metal, and the products produced by the general spray-free plastic preparation process have poor metallic texture and dull color, a metallic texture PBT composite material and its preparation equipment and preparation method are provided.

[0006] A metallic texture PBT composite material, composed of the following raw materials in mass fraction:

[0007] PBT resin 25-79 parts;

[0008] PET resin 5-42 parts;

[0009] 2 to 8 parts of toughening agent;

[0010] 0.3-1 part of anti-floating agent;

[0011] 10-40 parts of glass fiber powder;

[0012] 1 to 5 parts of spray-free functional pigment;

[0013] Nucleating agent 0.1-0.3 parts;

[0014] 0.2-0.6 parts of hindered phenol antioxidant;

[0015] 0.2-0.6 parts of phosphate antioxidant;

[0016] The glass fiber powder has a fiber diameter of 8-17 μm and a length of 50-200 μm.

[0017] Furthermore, the intrinsic viscosity of the PBT resin is 0.85-1.0 dL / g, and the intrinsic viscosity of the PET resin is 0.68-0.85 dL / g.

[0018] Furthermore, the toughening agent is at least one of Arkema AX8900 and DuPont 4170.

[0019] Furthermore, the anti-floating fiber agent is at least one of Xingtai Guoguang TAF, Clariant E vinegar, and Clariant OP vinegar.

[0020] Furthermore, the spray-free functional pigment is a surface-coated metal pigment, which includes a metal pigment layer and a transparent polymer layer, wherein the transparent polymer layer is wrapped around the outside of the metal pigment layer, and the surface of the transparent polymer layer has -GMA active groups.

[0021] Furthermore, the method for preparing the surface coating layer metallic pigment comprises the following steps:

[0022] 1) Pour 100 parts by mass of metallic pigment, 4 parts by mass of methyl methacrylate and 6 parts by mass of glycidyl methacrylate into a heated and stirred reaction kettle, and stir well to fully wet the metallic pigment;

[0023] 2) Add a small amount of initiator benzoyl peroxide at 50-80°C to fully polymerize the organic molecules on the surface of the metal pigment to obtain a spray-free functional pigment with a transparent polymer layer with self-GMA active groups on the surface.

[0024] A preparation device for a metallic-texture PBT composite material comprises a twin-screw extruder, wherein a barrel is provided in the twin-screw extruder, a twin-screw is rotatably sleeved in the barrel, a feed port, a first side feeding port, a second side feeding port and a vacuum port are sequentially connected on the barrel, a plurality of groups of shearing and kneading blocks are arranged between the corresponding feed port and the second side feeding port on the twin-screw, and a conveying-type plasticizing thread is arranged between the corresponding second side feeding port and the vacuum port on the twin-screw.

[0025] Furthermore, more than 4 groups of shearing and kneading blocks are arranged between the feed port and the first side feeding port, and 2-4 groups of shearing and kneading blocks are arranged between the first side feeding port and the second side feeding port.

[0026] A method for preparing a metallic texture PBT composite material comprises the following steps:

[0027] 1) PBT resin, PET resin, toughening agent and anti-floating agent weighed in proportion are added into a twin-screw extruder, and the above components are completely plasticized into a plastic melt by using the shear kneading block and heating in the twin-screw extruder;

[0028] 2) Add glass fiber powder to the plastic melt, and use a shear kneading block to stir and disperse the glass fiber powder in the plastic melt;

[0029] 3) adding the surface coating layer metal pigment, nucleating agent, hindered phenol antioxidant and phosphate antioxidant weighed in proportion into a low-speed stirring barrel and mixing them into a mixture, then adding the mixture into the plastic melt obtained in step 2), and using the conveying plasticizing screw in the twin-screw extruder to mix and extrude the mixture and the plastic melt to obtain a metallic texture PBT composite material;

[0030] 4) The metallic PBT composite material is successively subjected to water cooling, drying, and pelletizing by a pelletizer to obtain the final product.

[0031] Furthermore, in step 3), the mixed extrusion temperature of the mixture and the plastic melt is 220-260°C.

[0032] The advantages of the present invention are:

[0033] 1. The PBT composite material produced has bright colors, pearlescent luster and metallic texture;

[0034] 2. The PBT composite material is resistant to high temperature and has high strength, and has strong performance;

[0035] 3. Compared with the spray-free plastics on the market, it takes into account both performance and aesthetics, and the product quality is stable;

[0036] 4. The preparation equipment, preparation conditions and preparation method are easy to implement, facilitating long-term stable production;

[0037] 5. The preparation cost is low and the raw materials are easily available. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0039] Figure 1 This is a schematic diagram of the structure of the equipment for preparing metallic texture PBT composite materials.

[0040] Figure ID:

[0041] 1. Twin-screw extruder; 101. Cylinder; 2. Twin-screw; 201. Shearing and kneading block; 202. Conveying plasticizing thread; 3. Feed port; 4. First side feeding port; 5. Second side feeding port; 6. Vacuum port; 7. Heating module. DETAILED DESCRIPTION

[0042] In order to solve the problem that there is a lack of solutions on the market for producing spray-free engineering plastics with good metallic texture, high temperature resistance and close to the hardness of metal, and the products produced by the general spray-free plastic preparation process have poor metallic texture and dull color, a metallic texture PBT composite material and its preparation equipment and preparation method are provided.

[0043] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0044] It should be noted that the terms such as "within", "in" and "one" etc. cited in this specification are only for the convenience of description and are not used to limit the scope of the present invention. Changes or adjustments in their relative relationships, without substantially changing the technical content, should also be regarded as the scope of the present invention, and it is necessary to make it clear in advance.

[0045] In the description of the present invention, it should be understood that the terms "upper", "lower", "front", "rear", "left", "right", "vertical", "horizontal", etc. indicate the orientation or position relationship based on the orientation or position relationship shown in the drawings, which is only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", etc. are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first", "second", etc. may explicitly or implicitly include one or more of the features. In the description of the present invention, it should be noted that, unless otherwise clearly specified and defined, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be directly connected, or indirectly connected through an intermediate medium, or it can be the internal communication of two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the present invention can be understood by specific circumstances.

[0046] like Figure 1 As shown,

[0047] A metallic texture PBT composite material, composed of the following raw materials in mass fraction:

[0048] PBT resin 25-79 parts;

[0049] PET resin 5-42 parts;

[0050] 2 to 8 parts of toughening agent;

[0051] 0.3-1 part of anti-floating agent;

[0052] 10-40 parts of glass fiber powder;

[0053] 1 to 5 parts of spray-free functional pigment;

[0054] Nucleating agent 0.1-0.3 parts;

[0055] 0.2-0.6 parts of hindered phenol antioxidant;

[0056] 0.2-0.6 parts of phosphate antioxidant;

[0057] The fiber diameter of the glass fiber powder is 8-17 μm and the length is 50-200 μm. Compared with the traditional long fiber or short fiber, the glass fiber powder is relatively short and will not significantly increase the melt viscosity, thereby reducing the damage to the metal pigment flake structure caused by excessive melt viscosity.

[0058] Furthermore, the intrinsic viscosity of the PBT resin is 0.85-1.0 dL / g, and the intrinsic viscosity of the PET resin is 0.68-0.85 dL / g. The resin melt viscosity is medium to low, and the shear damage to the metal pigment is relatively weak, and the flaky structure of the metal pigment can be maintained well.

[0059] Furthermore, the toughening agent is at least one of Arkema AX8900 and DuPont 4170. These toughening agents have good toughening effect, low melt viscosity, and relatively weak shear damage to metal pigments.

[0060] Furthermore, the anti-floating fiber agent is at least one of Xingtai Guoguang TAF, Clariant E vinegar, and Clariant OP vinegar, which can have a good surface appearance effect on both glass fiber powder and metal pigment.

[0061] Furthermore, the spray-free functional pigment is a surface-coated metal pigment, which includes a metal pigment layer and a transparent polymer layer, wherein the transparent polymer layer is wrapped around the outside of the metal pigment layer, and the surface of the transparent polymer layer has -GMA active groups.

[0062] The preparation method of the surface coating layer metallic pigment comprises the following steps:

[0063] 1) Pour 100 parts by mass of metallic pigment, 4 parts by mass of methyl methacrylate and 6 parts by mass of glycidyl methacrylate into a heated and stirred reaction kettle, and stir well to fully wet the metallic pigment;

[0064] 2) Add a small amount of initiator benzoyl peroxide at 50-80°C to fully polymerize the organic molecules on the surface of the metal pigment to obtain a spray-free functional pigment with a transparent polymer layer with self-GMA active groups on the surface.

[0065] Since the surface layer of the spray-free functional pigment is a transparent polymer material, it has no effect on the optical appearance of the metal and can effectively protect the metal pigment from being damaged during the extrusion process. At the same time, the polymer material in the surface layer has its own -GMA active group and has good compatibility with PBT or PET. It effectively solves the problem of surface flow marks on injection molded products.

[0066] A preparation device for a metallic-texture PBT composite material comprises a twin-screw extruder 1, wherein the twin-screw extruder 1 is provided with a barrel 101, wherein a twin screw 2 is rotatably sleeved in the barrel 101, wherein a feed port 3, a first side feeding port 4, a second side feeding port 5 and a vacuum port 6 are sequentially connected to the barrel, wherein a plurality of groups of shearing and kneading blocks 201 are provided between the corresponding feed port 3 and the second side feeding port 4 on the twin screw 2, and a conveying-type plasticizing thread 202 is provided between the corresponding second side feeding port 5 and the vacuum port 6 on the twin screw 2.

[0067] Furthermore, more than 4 groups of shearing and kneading blocks 201 are arranged between the feed port 3 and the first side feeding port 4 , and 2-4 groups of shearing and kneading blocks 201 are arranged between the first side feeding port 4 and the second side feeding port 5 .

[0068] There are no less than 4 sets of shearing and kneading blocks 201 between the feed port 3 and the first side feed port 4, ensuring that the plastic components such as PBT resin, PET resin, toughening agent, etc. are completely plasticized into melt through this section. There are 2 to 4 sets of shearing and kneading blocks 201 between the first side feed port and the second side feed port, which only need to ensure the dispersion of glass fiber powder in the plastic melt. There is no need for shearing and kneading blocks 201 between the second side feed port 5 and the vacuum port 6, and all are conveying type plasticizing threads 202, which prevents the surface coating layer metal pigment from being crushed by the shearing and kneading blocks 202.

[0069] It is also worth mentioning that a heating module 7 is disposed on the surface of the twin-screw extruder 1 .

[0070] A method for preparing a metallic texture PBT composite material comprises the following steps:

[0071] 1) PBT resin, PET resin, toughening agent and anti-floating agent weighed in proportion are added to the feed port 3 of the twin-screw extruder 1, and the above components are completely plasticized into a plastic melt by using the shearing and kneading block 201 and heating in the twin-screw extruder 1;

[0072] 2) adding glass fiber powder into the plastic melt through the first side feeding port 4, and stirring and dispersing the glass fiber powder into the plastic melt by using the shear kneading block 201;

[0073] 3) adding the surface coating layer metal pigment, nucleating agent, hindered phenol antioxidant and phosphate antioxidant weighed in proportion to a low-speed stirring barrel and mixing them into a mixture, then adding the mixture into the plastic melt obtained in step 2) through the second side feeding port 5, mixing the mixture and the plastic melt by using the conveying plasticizing screw 202 in the twin-screw extruder 1, and extruding at a temperature of 220-260° C. to obtain a metallic texture PBT composite material;

[0074] 4) The metallic PBT composite material is successively subjected to water cooling, drying, and pelletizing by a pelletizer to obtain the final product.

[0075] The present invention is further described in detail below by means of specific examples. Unless otherwise specified, the raw materials used in the examples can be obtained from conventional commercial sources.

[0076] The raw material compositions of the metallic PBT composite materials of Comparative Example 1 and Examples 1 to 5 are shown in Table 1 below.

[0077] Table 1 Raw material composition of the metallic PBT composite material of Comparative Example 1 and Examples 1 to 5

[0078] raw material Comparative Example 1 Example 1 Example 2 Example 3 Example 4 Example 5 PBT resin 32.5 32.5 42.5 31 32.5 62.5 PET resin 30 30 20 20 30 10 Toughening agent 4 4 4 3 4 6 Anti-floating agent 0.6 0.6 0.5 0.8 0.6 0.4 Glass fiber powder 30 30 30 40 30 20 Spray-free functional pigments 2 2 2 4 2 4 Nucleating Agent 0.3 0.3 0.2 0.2 0.3 0.1 Hindered phenol antioxidant 0.3 0.3 0.3 0.5 0.5 0.2 Phosphate Antioxidant 0.3 0.3 0.3 0.5 0.5 0.2

[0079] The raw materials used in Table 1 are described as follows:

[0080] In Comparative Example 1,

[0081] PBT resin: TH6083 (Tunhe, Xinjiang);

[0082] PET resin: FG600 (Yizheng Chemical Fiber);

[0083] Toughening agent: AX8900 (Arkema);

[0084] Anti-floating agent: TAF (Xingtai Guoguang);

[0085] Glass fiber powder: (Shandong Taishan Fiberglass);

[0086] Spray-free functional pigments: metallic pigments without surface treatment;

[0087] Nucleating agent: Nav101;

[0088] Hindered phenol antioxidant: 1010;

[0089] Phosphate antioxidant: 168.

[0090] The difference between Examples 1-3 and Comparative Example 1 is that:

[0091] Spray-free functional pigments: homemade surface coating metallic pigments.

[0092] The difference between Example 4 and Examples 1-3 is that:

[0093] PBT resin: 1100 (China Blue Morning Light);

[0094] PET resin: CB-608S (Sanfangxiang);

[0095] Toughening agent: 4170 (DuPont);

[0096] Anti-floating agent: OP wax (Clariant);

[0097] Glass fiber powder: (Chongqing International Composite Materials).

[0098] The difference between Example 5 and Examples 1-3 is that:

[0099] PBT resin: 1100 (China Blue Morning Light);

[0100] PET resin: CB-608S (Sanfangxiang);

[0101] Anti-floating agent: E wax (Clariant);

[0102] Glass fiber powder: (Chongqing International Composite Materials).

[0103] Combined with Figure 1 To illustrate, Comparative Example 1 was prepared according to the following method:

[0104] The glass fiber powder is weighed according to the above ratio and enters the twin screw extruder 1 from the first side feed port 3, and the other component mixtures are all entered from the feed port 3. Under the extrusion working condition of 250°C, the final product is obtained through twin screw extrusion, strand water cooling, blow drying, and pelletizing by a pelletizer.

[0105] In Examples 1 to 5, the finished products were obtained according to the above-mentioned method for preparing the metallic PBT composite material at 240° C. extrusion conditions.

[0106] After the finished product was baked at 140°C for 3 hours, it was made into ISO standard specimens through an injection molding machine. After cooling for 24 hours in a constant temperature environment of 23°C, various performance data were measured and its metallic texture was evaluated.

[0107] The test properties of the metallic PBT composite materials of Comparative Example 1 and Examples 1 to 5 are shown in Table 2 below.

[0108] Table 2 Test performance of the metallic PBT composite materials of Comparative Example 1 and Examples 1 to 5

[0109]

[0110] The test standards or methods for each performance indicator in Table 2 are as follows:

[0111] Density: ISO1183;

[0112] Tensile strength: ISO527-2;

[0113] Flexural modulus: ISO178;

[0114] Izod notched impact strength: ISO180;

[0115] Heat deformation temperature (1.82MPa): ISO75-2

[0116] Color palette texture: visual sense.

[0117] As can be seen from Table 2, compared with Comparative Example 1, Examples 1 to 5 can significantly improve the texture of the color plate by using a unique preparation method and a surface coating layer of metallic pigments, and the texture of the color plate will not be affected by differences in other components.

[0118] In addition, the amount of glass fiber powder used has a strong positive correlation with various performance indicators, and the positive correlation between the amount of PET resin used and various performance indicators is also quite obvious.

[0119] The above contents are further detailed descriptions of the present invention in combination with specific preferred implementation modes. It cannot be considered that the specific implementation of the present invention is limited to these descriptions. That is, all equivalent changes and modifications made within the scope of this application should still fall within the scope of the present invention.

Claims

1. A metallic texture PBT composite material, characterized in that: It is composed of the following raw materials by mass fraction: PBT resin 25~79 parts; PET resin 5~42 parts; 2~8 parts of toughening agent; 0.3~1 part of anti-floating agent; 10~40 parts of glass fiber powder; 1~5 parts of spray-free functional pigment; Nucleating agent 0.1~0.3 parts; Hindered phenol antioxidant 0.2~0.6 parts; 0.2~0.6 parts of phosphate antioxidant; The glass fiber powder has a fiber diameter of 8-17 μm and a length of 50-200 μm.

2. The metallic texture PBT composite material according to claim 1, characterized in that: The intrinsic viscosity of the PBT resin is 0.85-1.0 dL / g, and the intrinsic viscosity of the PET resin is 0.68-0.85 dL / g.

3. The metallic texture PBT composite material according to claim 1, characterized in that: The toughening agent is at least one of Arkema AX8900 and DuPont 4170.

4. The metallic texture PBT composite material according to claim 1, characterized in that: The anti-floating fiber agent is at least one of Xingtai Guoguang TAF, Clariant E vinegar and Clariant OP vinegar.

5. The metallic texture PBT composite material according to claim 1, characterized in that: The spray-free functional pigment is a surface-coated metal pigment, which includes a metal pigment layer and a transparent polymer layer. The transparent polymer layer is wrapped around the outside of the metal pigment layer, and the surface of the transparent polymer layer has -GMA active groups.

6. The metallic texture PBT composite material according to claim 5, characterized in that: The preparation method of the surface coating layer metallic pigment comprises the following steps: 1) Pour 100 parts by mass of metallic pigment, 4 parts by mass of methyl methacrylate and 6 parts by mass of glycidyl methacrylate into a heated and stirred reactor, and stir well to fully wet the metallic pigment; 2) At 50-80°C, add a small amount of initiator benzoyl peroxide to fully polymerize the organic molecules on the surface of the metal pigment to obtain a spray-free functional pigment with a transparent polymer layer with its own -GMA active groups on the surface.

7. A preparation device for a metallic PBT composite material, applied to the metallic PBT composite material described in any one of claims 1 to 6, characterized in that: The invention comprises a twin-screw extruder, wherein a barrel is provided in the twin-screw extruder, a twin-screw is rotatably sleeved in the barrel, a feed port, a first side feeding port, a second side feeding port and a vacuum port are sequentially connected on the barrel, a plurality of groups of shearing and kneading blocks are arranged between the corresponding feed port and the second side feeding port on the twin-screw, and a conveying type plasticizing thread is arranged between the corresponding second side feeding port and the vacuum port on the twin-screw.

8. The preparation equipment of the metallic texture PBT composite material according to claim 7, characterized in that: More than 4 groups of shearing and kneading blocks are arranged between the feed port and the first side feed port, and 2-4 groups of shearing and kneading blocks are arranged between the first side feed port and the second side feed port.

9. A method for preparing a metallic PBT composite material, applied to the metallic PBT composite material described in any one of claims 1 to 6, characterized in that: The following steps are involved: 1) PBT resin, PET resin, toughening agent and anti-floating agent weighed in proportion are added into a twin-screw extruder, and the shear kneading block and heating in the twin-screw extruder are used to completely plasticize the above components into a plastic melt; 2) Add glass fiber powder to the plastic melt, and use a shear kneading block to stir and disperse the glass fiber powder in the plastic melt; 3) adding the surface coating layer metal pigment, nucleating agent, hindered phenol antioxidant and phosphate antioxidant weighed in proportion into a low-speed stirring barrel and mixing them into a mixture, then adding the mixture into the plastic melt obtained in step 2), and using the conveying plasticizing screw in the twin-screw extruder to mix and extrude the mixture and the plastic melt to obtain a metallic texture PBT composite material; 4) The metallic PBT composite material is successively subjected to water cooling, drying and pelletizing by a pelletizer to obtain the final product.

10. The method for preparing the metallic texture PBT composite material according to claim 9, characterized in that: In step 3), the mixed extrusion temperature of the mixture and the plastic melt is 220-260°C.

Citation Information

Patent Citations

  • Spraying-free imitative metal PBT and preparation method thereof

    CN104140655A

  • Preparation method for resin with free-spraying metal effect

    CN105237937A

  • Coating-free glass fiber reinforced PBT / PET composition having metal effect and preparation method thereof

    CN109096706A

  • PBT / PET alloy material and preparation method thereof

    CN109486136A

  • Double-screw extruder and preparation method of high-load polyolefin master batch

    CN117227138A