Anti-aging amorphous copolyester material and preparation method thereof
By introducing double bond groups and glass flakes into PETG materials, the problem of poor oxidation resistance under ultraviolet light is solved, the UV resistance and mechanical properties are improved, and better flexibility and corrosion resistance are achieved.
Patent Information
- Application Number
- CN202411235449.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-12
AI Technical Summary
The existing PETG materials have poor antioxidant properties under ultraviolet light, resulting in poor mechanical properties, limiting their application range, and conventional ultraviolet absorbers are volatile and have poor compatibility.
By introducing double bond groups into PETG materials, reacting with a polymeric UV absorber using acrylic acid-modified 2-hydroxyterephthalic acid, introducing UV absorber, and adding glass flakes to PETG to improve UV resistance and mechanics performance.
It significantly improves the UV resistance and mechanical properties of PETG materials, reduces crystallinity, enhances flexibility and chemical corrosion resistance, and improves compatibility with PETG materials.
Smart Images

Figure BDA0005027606970000101 
Figure BDA0005027606970000111
Abstract
Description
Technical Field
[0001] The invention relates to the field of copolyester materials, and in particular to an anti-aging non-crystalline copolyester material and a preparation method thereof. Background Art
[0002] Polyethylene terephthalate (PET) refers to a high molecular polymer obtained by esterification and polymerization of terephthalic acid (PTA) and ethylene glycol (EG). It can maintain excellent dimensional stability and physical properties in a wide temperature range, and is therefore widely used in the production of fibers and engineering plastics. Although PET has many excellent properties, its molecules contain rigid benzene rings and are highly symmetrical and unbranched, resulting in poor flexibility.
[0003] Copolyester (PETG) obtained by esterification and polycondensation by adding monomers such as neopentyl glycol (NPG) and 1,4-cyclohexanedimethanol (CHDM) is a new type of polymer material. Compared with PET, PETG has a lower crystallization ability and a wider processing window, which broadens the application market of polyester products. For CHDM-modified PET, copolyester materials can be divided into two categories according to the different CHDM content of the monomer. PETG has a CHDM content of less than 50%, and PCTG has a CHDM content of more than 50%. Among them, PETG has good transparency, plasticity and chemical stability, and is widely used in the field of food packaging materials. However, PETG materials still have poor antioxidant properties and the problem that molecular segments are easily broken under ultraviolet light, which makes the mechanical properties of PETG materials worse and limits its application range. Therefore, it is very important to improve the anti-aging properties of PETG materials.
[0004] Patent CN113429758A discloses a hydrolysis-resistant and anti-aging PET modified material and a preparation method thereof. The anti-aging performance of the PET modified material is improved by adding nano-titanium dioxide and nano-silicon dioxide. However, nano-titanium dioxide and nano-silicon dioxide are prone to agglomeration during the PET processing and have poor compatibility with the PET modified material.
[0005] Patent CN105086386A discloses a PET composite material, which uses bentonite modified with aminobenzoic acid and aminocaproic acid to improve the UV resistance of the PET composite material. However, bentonite is hygroscopic and may affect the moisture resistance of the PET composite material.
[0006] Therefore, there is an urgent need in the market for a non-crystalline copolyester material with good UV resistance and aging resistance. Summary of the invention
[0007] In view of the problems existing in the prior art, the purpose of the present invention is to obtain a non-crystalline copolyester material with good UV resistance and aging resistance.
[0008] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0009] On one hand, the present invention provides an anti-aging non-crystalline copolyester material, which comprises the following raw materials in parts by weight: 30-50 parts of modified PETG, 10-15 parts of fillers, 3-5 parts of flame retardants, and 0.5-1 parts of antioxidants.
[0010] In some embodiments, the method for preparing the modified PETG comprises the following steps:
[0011] A1. Add 2-hydroxyterephthalic acid, acrylic acid and tetraisopropyl titanate into a reaction vessel, and react at 70-80° C. for 1-2 hours to obtain terephthalic acid containing a double bond;
[0012] A2, adding the double-bond-containing terephthalic acid obtained in step A1, a polymeric ultraviolet light absorber and dibenzoyl peroxide into a reaction vessel, and reacting at 80-90° C. for 2-4 hours to obtain terephthalic acid containing ultraviolet light absorbing segments;
[0013] A3. Add terephthalic acid containing ultraviolet light absorbing segments obtained in step A2, terephthalic acid, ethylene glycol, 1,4-cyclohexanedimethanol, neopentyl glycol and germanium dioxide into a reaction vessel, heat to 240-260° C., react at 0.2-0.3 MPa, adjust the pressure to 95-105 Pa when the water output reaches 99.3-99.7% of the theoretical water output value, heat to 270-290° C., react for 2-3 hours, and obtain modified PETG.
[0014] Preferably, the preparation method of the modified PETG comprises the following steps:
[0015] A1. Add 2-hydroxyterephthalic acid, acrylic acid and tetraisopropyl titanate into a reaction vessel, wherein the mass ratio of 2-hydroxyterephthalic acid to acrylic acid is (1.5-2.0):1, and react at 70-80° C. for 1-2 hours to obtain terephthalic acid containing a double bond;
[0016] A2, adding the double-bond-containing terephthalic acid obtained in step A1, a polymeric ultraviolet light absorber and dibenzoyl peroxide into a reaction vessel, and reacting at 80-90° C. for 2-4 hours to obtain terephthalic acid containing ultraviolet light absorbing segments;
[0017] A3. Add terephthalic acid containing ultraviolet light absorbing segments obtained in step A2, terephthalic acid, ethylene glycol, 1,4-cyclohexanedimethanol, neopentyl glycol and germanium dioxide into a reaction vessel, heat to 240-260° C., react at 0.2-0.3 MPa, adjust the pressure to 95-105 Pa when the water output reaches 99.3-99.7% of the theoretical water output value, heat to 270-290° C., react for 2-3 hours, and obtain modified PETG.
[0018] In order to improve the anti-aging performance of PETG materials, it is conventional to add ultraviolet absorbers, but conventional ultraviolet absorbers are easy to volatilize and have poor compatibility with PETG, and there is a problem of easy precipitation. To address this problem, this application introduces double bond groups on PETG by using acrylic acid to modify 2-hydroxyterephthalic acid and then using it as a reactant to participate in the esterification reaction, so that it can react with polymeric ultraviolet absorbers, successfully introduce ultraviolet absorbing groups on the PETG chain segments, and improve the anti-ultraviolet performance of PETG materials. In addition, the crystallinity of PETG materials is further reduced, which may be because the introduction of side chains destroys the regularity of the PETG chain segments, making the PETG chain segments difficult to crystallize.
[0019] In some embodiments, the polymeric ultraviolet absorber is 2-hydroxy-4-methacryloxybenzophenone or 2-hydroxy-4-allyloxybenzophenone.
[0020] Preferably, the polymeric ultraviolet absorber is 2-hydroxy-4-methacryloyloxybenzophenone.
[0021] The present application prefers 2-hydroxy-4-methacryloyloxybenzophenone as a polymeric ultraviolet absorber to participate in the reaction of terephthalic acid containing double bonds to make the PETG material have better ultraviolet resistance. This may be because 2-hydroxy-4-methacryloyloxybenzophenone contains ester bond groups, which are easily attracted by the polyester groups on the main chain, thereby more effectively preventing ultraviolet rays from destroying the ester bonds on the PETG main chain.
[0022] In some embodiments, the mass ratio of the double-bond-containing terephthalic acid to the polymeric ultraviolet absorber in step A2 is 1:(0.7-0.9).
[0023] The present application can make the PETG material have better UV resistance and mechanical properties by selecting a polymeric UV absorber with a specific ratio as a modifier. This may be because the UV absorbing groups can be evenly distributed on the PETG main chain, and self-polymerization is not easy to occur, so that each part of the PETG material has good UV resistance, and there is no excess polymeric UV absorber remaining in the system, which will not affect the mechanical properties of the PETG material.
[0024] In some embodiments, the mass ratio of ethylene glycol, terephthalic acid, terephthalic acid containing ultraviolet light absorbing segments, 1,4-cyclohexanedimethanol and neopentyl glycol in step A3 is (1.3-1.6):(2.4-2.7):(0.5-0.7):0.5:0.5.
[0025] The asymmetry brought by 1,4-cyclohexanedimethanol, neopentyl glycol and ultraviolet absorption molecular chains can reduce the crystallinity of PETG and improve its flexibility. However, the introduction of 1,4-cyclohexanedimethanol and ultraviolet absorption molecular chains will also increase the rigid groups in the system, such as cyclohexane and benzene ring groups, affecting the flexibility of PETG. The present application limits the ratio of terephthalic acid, ethylene glycol, terephthalic acid containing ultraviolet absorption segments and 1,4-cyclohexanedimethanol, so as to not only make PETG copolyester have non-crystalline properties, but also ensure its mechanical properties.
[0026] In some embodiments, the filler is one or more of titanium dioxide, calcium carbonate, and barium sulfate.
[0027] Preferably, the filler is titanium dioxide.
[0028] In some embodiments, the flame retardant is one or more of a phosphorus-based flame retardant, an organosilicon flame retardant, and an intumescent flame retardant.
[0029] Preferably, the flame retardant is a phosphorus-based flame retardant.
[0030] More preferably, the flame retardant is triphenyl phosphate.
[0031] In some embodiments, the antioxidant is a combination of one or more of hindered phenols, phosphites, thioesters, benzofurans, and hydroxylamine antioxidants.
[0032] Preferably, the antioxidant is a hindered phenol antioxidant.
[0033] More preferably, the antioxidant is antioxidant 1010.
[0034] In some embodiments, the anti-aging non-crystalline copolyester material further contains 5-7 parts by weight of modified glass flakes.
[0035] In some embodiments, the method for preparing the modified glass flakes comprises the following steps:
[0036] B1. Add glass flakes and N,N-dimethylformamide to a reaction vessel, perform ultrasonication for 30-60 minutes, add isocyanate, stir at 60-70° C. for 2-4 hours, cool to room temperature, wash with anhydrous ethanol for 3-5 times, filter, and dry to obtain activated glass flakes;
[0037] B2. Add the activated glass flakes obtained in step B1, N,N-dimethylformamide and 2-hydroxy-4-(2,3-epoxypropoxy)benzophenone into a reaction vessel, heat to 60-70°C, and stir for 2-3 hours to obtain modified glass flakes.
[0038] By adding glass flakes to the PETG material, the present application can further improve the chemical corrosion resistance and UV resistance of the PETG material. This is because the glass flakes are arranged in an overlapping manner in the PETG material, isolating the corrosive substances from the substrate, reducing the contact area between the corrosive substances and the substrate, thereby reducing the corrosive effect of the corrosive substances on the substrate, and the glass flakes themselves can shield ultraviolet wavelengths.
[0039] The present application introduces NCO groups on the glass flakes so that they can react with 2-hydroxy-4-(2,3-epoxypropoxy)benzophenone. On the one hand, the lower-cost 2-hydroxy-4-(2,3-epoxypropoxy)benzophenone is introduced into the PETG material, which can further improve the anti-aging properties of the PETG material. On the other hand, organic chain segments are introduced into the glass flakes to increase their compatibility in the PETG material.
[0040] In some embodiments, the mass ratio of the glass flakes to the isocyanate in step B1 is (1-3):1.
[0041] In some embodiments, the mass ratio of the activated glass flakes to 2-hydroxy-4-(2,3-epoxypropoxy)benzophenone in step B2 is (2-4):1.
[0042] The applicant can make the glass flakes have good activation properties by selecting a specific ratio of isocyanate to react with the hydroxyl groups on the surface of the glass flakes, and can further improve the mechanical properties of PETG by selecting a specific ratio of 2-hydroxy-4-(2,3-epoxypropoxy)benzophenone to react with the activated glass flakes. This may be because the glass flakes contain multiple -NCO groups that have not reacted with 2-hydroxy-4-(2,3-epoxypropoxy)benzophenone, which can promote the formation of a cross-linked network structure inside the copolyester and improve its mechanical properties and corrosion resistance.
[0043] Another aspect of the present invention provides a method for preparing an anti-aging non-crystalline copolyester material, comprising the following steps:
[0044] S1. Mix the modified PETG, filler, flame retardant and antioxidant, add them into a mixer, and mix for 10-30 minutes to obtain a premix;
[0045] S2. The premix obtained in step S1 is put into a twin-screw extruder, extruded from a die head, and pelletized. The extrusion temperature is controlled at 210-220° C. to obtain an anti-aging non-crystalline copolyester material.
[0046] Compared with the prior art, the present invention has the following beneficial effects:
[0047] (1) The present invention blends modified PET with fillers, flame retardants, and antioxidants to obtain an anti-aging non-crystalline copolyester material with good corrosion resistance and mechanical properties.
[0048] (2) The present invention introduces double bond groups into PETG by using acrylic acid to modify 2-hydroxyterephthalic acid and then using it as a reactant in an esterification reaction, so that it can react with a polymeric ultraviolet absorber, successfully introducing ultraviolet absorbing groups into the PETG chain segments, thereby improving the anti-ultraviolet performance of the PETG material, and further reducing the crystallinity of the PETG material, thereby improving the flexibility of the PETG.
[0049] (3) The present invention adds glass flakes to the PETG material and introduces NCO groups on the glass flakes so that the glass flakes can react with 2-hydroxy-4-(2,3-epoxypropoxy)benzophenone. On the one hand, the lower-cost 2-hydroxy-4-(2,3-epoxypropoxy)benzophenone is introduced into the PETG material, which can further improve the chemical corrosion resistance and UV resistance of the PETG material. On the other hand, the organic chain segments are introduced into the glass flakes, which increases its compatibility with the PETG material. DETAILED DESCRIPTION
[0050] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0051] In the following examples and comparative examples, except for modified PETG, modified glass flakes and 2-hydroxy-4-(2,3-epoxypropoxy)benzophenone, the other compounds and related reagents used can be purchased from the market. The particle size of the glass flakes is 40 mesh, which was purchased from Hebei Lichen Anticorrosive Coatings Co., Ltd.
[0052] Preparation Example 1
[0053] The preparation method of modified PETG-1 comprises the following steps:
[0054] A1. Add 1.7 g of 2-hydroxyterephthalic acid, 1 g of acrylic acid and 0.0015 g of tetraisopropyl titanate into a reaction vessel, and react at 75° C. for 1.5 h to obtain terephthalic acid containing a double bond;
[0055] A2, adding 2.5 g of terephthalic acid containing double bonds obtained in step A1, 2 g of 2-hydroxy-4-methacryloyloxybenzophenone and 0.1 g of dibenzoyl peroxide into a reaction container, reacting at 85° C. for 3 h to obtain terephthalic acid containing ultraviolet light absorbing segments;
[0056] A3, 0.6g of terephthalic acid containing ultraviolet light absorption segments obtained in step A2, 2.5g of terephthalic acid, 1.4g of ethylene glycol, 0.5g of 1,4-cyclohexanedimethanol, 0.5g of neopentyl glycol and 0.1g of germanium dioxide were added to a reaction container, the temperature was raised to 250°C, and the reaction was carried out at 0.3MPa. When the water output reached 99.5% of the theoretical water output value, the pressure was adjusted to 100Pa, the temperature was raised to 280°C, and the reaction was carried out for 2h to obtain modified PETG-1.
[0057] Preparation Example 2
[0058] The preparation method of modified PETG-2 comprises the following steps:
[0059] A1. Add 1.7 g of 2-hydroxyterephthalic acid, 1 g of acrylic acid and 0.0015 g of tetraisopropyl titanate into a reaction vessel, and react at 75° C. for 1.5 h to obtain terephthalic acid containing a double bond;
[0060] A2, adding 2.5 g of terephthalic acid containing double bonds obtained in step A1, 2.5 g of 2-hydroxy-4-methacryloyloxybenzophenone and 0.1 g of dibenzoyl peroxide into a reaction container, reacting at 85° C. for 3 h to obtain terephthalic acid containing ultraviolet light absorbing segments;
[0061] A3, 0.6g of terephthalic acid containing ultraviolet light absorption segments obtained in step A2, 2.5g of terephthalic acid, 1.4g of ethylene glycol, 0.5g of 1,4-cyclohexanedimethanol, 0.5g of neopentyl glycol and 0.1g of germanium dioxide were added to a reaction container, the temperature was raised to 250°C, and the reaction was carried out at 0.3MPa. When the water output reached 99.5% of the theoretical water output value, the pressure was adjusted to 100Pa, the temperature was raised to 280°C, and the reaction was carried out for 2h to obtain modified PETG-2.
[0062] Preparation Example 3
[0063] The preparation method of modified PETG-3 comprises the following steps:
[0064] A1. Add 1.7 g of 2-hydroxyterephthalic acid, 1 g of acrylic acid and 0.0015 g of tetraisopropyl titanate into a reaction vessel, and react at 75° C. for 1.5 h to obtain terephthalic acid containing a double bond;
[0065] A2, adding 2.5 g of terephthalic acid containing double bonds obtained in step A1, 2 g of 2-hydroxy-4-methacryloyloxybenzophenone and 0.1 g of dibenzoyl peroxide into a reaction container, reacting at 85° C. for 3 h to obtain terephthalic acid containing ultraviolet light absorbing segments;
[0066] A3. Add 1 g of terephthalic acid containing an ultraviolet light absorbing segment obtained in step A2, 2.5 g of terephthalic acid, 2 g of ethylene glycol, 0.5 g of 1,4-cyclohexanedimethanol, 0.5 g of neopentyl glycol and 0.1 g of germanium dioxide into a reaction container, heat to 250 ° C, react at 0.3 MPa, adjust the pressure to 100 Pa when the water output reaches 99.5% of the theoretical water output value, heat to 280 ° C and react for 2 h to obtain modified PETG-3.
[0067] Preparation Example 4
[0068] The preparation method of PETG is as follows: 3.1g of terephthalic acid, 1.4g of ethylene glycol, 0.5g of 1,4-cyclohexanedimethanol, 0.5g of neopentyl glycol and 0.1g of germanium dioxide are added into a reaction container, the temperature is raised to 250°C, and the reaction is carried out at 0.3MPa. When the water output reaches 99.5% of the theoretical water output value, the pressure is adjusted to 100Pa, the temperature is raised to 280°C, and the reaction is carried out for 2h to obtain PETG.
[0069] Preparation Example 5
[0070] The preparation method of 2-hydroxy-4-(2,3-epoxypropoxy)benzophenone is as follows: 2.1 g of 2,4-dihydroxybenzophenone, 2.7 g of epichlorohydrin and 5 g of a 2 mol / L sodium hydroxide aqueous solution are added to a reaction container, the temperature is raised to 90° C. and the reaction is carried out for 4 hours to obtain 2-hydroxy-4-(2,3-epoxypropoxy)benzophenone.
[0071] Preparation Example 6
[0072] The preparation method of modified glass flake-1 comprises the following steps:
[0073] B1. Add 4 g of glass flakes and 10 g of N,N-dimethylformamide into a reaction vessel and perform ultrasonication for 40 min. Add 2 g of isophorone diisocyanate, stir at 65 °C for 3 h, cool to room temperature, wash 4 times with 10 g of anhydrous ethanol, filter and dry to obtain activated glass flakes.
[0074] B2. Add 3 g of activated glass flakes obtained in step B1, 5 g of N,N-dimethylformamide and 1 g of 2-hydroxy-4-(2,3-epoxypropoxy)benzophenone into a reaction vessel, heat to 65° C., and stir for 2.5 h to obtain modified glass flake-1.
[0075] Preparation Example 7
[0076] The preparation method of modified glass flake-2 comprises the following steps:
[0077] B1. Add 4 g of glass flakes and 10 g of N,N-dimethylformamide into a reaction vessel and perform ultrasonication for 40 min. Add 1 g of isophorone diisocyanate, stir at 65 °C for 3 h, cool to room temperature, wash 4 times with 10 g of anhydrous ethanol, filter and dry to obtain activated glass flakes.
[0078] B2. Add 3 g of activated glass flakes obtained in step B1, 5 g of N,N-dimethylformamide and 1 g of 2-hydroxy-4-(2,3-epoxypropoxy)benzophenone into a reaction vessel, heat to 65° C., and stir for 2.5 h to obtain modified glass flake-2.
[0079] Preparation Example 8
[0080] The preparation method of modified glass flake-3 comprises the following steps:
[0081] B1. Add 4 g of glass flakes and 10 g of N,N-dimethylformamide into a reaction vessel and perform ultrasonication for 40 min. Add 0.5 g of isophorone diisocyanate, stir at 65 ° C for 3 h, cool to room temperature, wash 4 times with 10 g of anhydrous ethanol, filter and dry to obtain activated glass flakes.
[0082] B2. Add 1 g of activated glass flakes obtained in step B1, 5 g of N,N-dimethylformamide and 1 g of 2-hydroxy-4-(2,3-epoxypropoxy)benzophenone into a reaction vessel, heat to 65°C, and stir for 2.5 hours to obtain modified glass flake-3.
[0083] Example 1
[0084] An anti-aging non-crystalline copolyester material comprises the following raw materials, measured in parts by weight: 40 parts of modified PETG-1, 12 parts of titanium dioxide, 4 parts of triphenyl phosphate, and 0.75 parts of antioxidant 1010.
[0085] The method for preparing the anti-aging non-crystalline copolyester material of this embodiment comprises the following steps:
[0086] S1. Mix modified PETG-1, titanium dioxide, triphenyl phosphate and antioxidant 1010, add into a mixer, and mix for 20 minutes to obtain a premix;
[0087] S2. The premix obtained in step S1 is put into a twin-screw extruder, extruded from a die head, and pelletized. The extrusion temperature is controlled at 215° C. to obtain an anti-aging non-crystalline copolyester material.
[0088] Example 2
[0089] An anti-aging non-crystalline copolyester material comprises the following raw materials, measured in parts by weight: 30 parts of modified PETG-1, 10 parts of titanium dioxide, 3 parts of triphenyl phosphate, and 0.5 parts of antioxidant 1010.
[0090] The method for preparing the anti-aging non-crystalline copolyester material of this embodiment comprises the following steps:
[0091] S1. Mix modified PETG-1, titanium dioxide, triphenyl phosphate and antioxidant 1010, add into a mixer, and mix for 10 minutes to obtain a premix;
[0092] S2. The premix obtained in step S1 is put into a twin-screw extruder, extruded from a die head, and pelletized. The extrusion temperature is controlled at 210° C. to obtain an anti-aging non-crystalline copolyester material.
[0093] Example 3
[0094] An anti-aging non-crystalline copolyester material comprises the following raw materials, measured in parts by weight: 50 parts of modified PETG-1, 15 parts of titanium dioxide, 5 parts of triphenyl phosphate, and 1 gram of antioxidant 1010.
[0095] The method for preparing the anti-aging non-crystalline copolyester material of this embodiment comprises the following steps:
[0096] S1. Mix modified PETG-1, titanium dioxide, triphenyl phosphate and antioxidant 1010, add into a mixer, and mix for 30 minutes to obtain a premix;
[0097] S2. The premix obtained in step S1 is put into a twin-screw extruder, extruded from a die head, and pelletized. The extrusion temperature is controlled at 220° C. to obtain an anti-aging non-crystalline copolyester material.
[0098] Example 4
[0099] An anti-aging non-crystalline copolyester material and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of modified PETG-1 is replaced by modified PETG-2.
[0100] Example 5
[0101] An anti-aging non-crystalline copolyester material and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the modified PETG-1 is replaced by modified PETG-3 in equal amounts.
[0102] Example 6
[0103] An anti-aging non-crystalline copolyester material comprises the following raw materials, measured in parts by weight: 40 parts of modified PETG-1, 12 parts of titanium dioxide, 4 parts of triphenyl phosphate, 0.75 parts of antioxidant 1010, and 6 parts of modified glass flake-1.
[0104] The method for preparing the anti-aging non-crystalline copolyester material of this embodiment comprises the following steps:
[0105] S1. Mix modified PETG-1, titanium dioxide, triphenyl phosphate, antioxidant 1010 and modified glass flake-1, add them into a mixer, and mix for 20 minutes to obtain a premix;
[0106] S2. The premix obtained in step S1 is put into a twin-screw extruder, extruded from a die head, and pelletized. The extrusion temperature is controlled at 215° C. to obtain an anti-aging non-crystalline copolyester material.
[0107] Example 7
[0108] An anti-aging non-crystalline copolyester material and a preparation method thereof. The specific implementation method is the same as Example 6, except that the modified glass flake-1 is replaced by modified glass flake-2 in equal amounts.
[0109] Example 8
[0110] An anti-aging non-crystalline copolyester material and a preparation method thereof. The specific implementation method is the same as Example 6, except that the modified glass flake-1 is replaced by modified glass flake-3 in equal amounts.
[0111] Example 9
[0112] An anti-aging non-crystalline copolyester material and a preparation method thereof. The specific implementation method is the same as Example 6, except that the modified glass flake-1 is replaced by glass flakes in equal amounts.
[0113] Comparative Example 1
[0114] An anti-aging non-crystalline copolyester material and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of modified PETG is replaced by PETG.
[0115] Performance Testing
[0116] The anti-aging non-crystalline copolyester materials obtained in the above embodiments and comparative examples were tested:
[0117] (1) Mechanical properties: The test method for the notched cantilever impact strength of the anti-aging non-crystalline copolyester material is ASTM D256, and the test temperature is 23°C; the test method for the breaking strength and breaking elongation is ASTM D638.
[0118] (2) Haze: The haze test method used for anti-aging non-crystalline copolyester materials is ASTM D1003.
[0119] (3) Anti-aging: The anti-aging performance test method of the non-crystalline copolyester material is GB / T16422.2-1999. The aging box is set at 60°C and 60% humidity. The irradiance of the light source with a wavelength between 290-800nm is 550W / m 2 .
[0120] (4) Corrosion resistance: The anti-aging non-crystalline copolyester material was cut into small pieces of 1 cm × 1 cm, soaked in 5 g of 60% sulfuric acid aqueous solution for 100 h, and then washed three times with 10 g of deionized water. After drying, the weight reduction rate was calculated: weight reduction rate = (initial weight - weight after drying) ÷ initial weight × 100%.
[0121] The test results are shown in Table 1:
[0122] Table 1
[0123]
[0124]
[0125] It can be seen from the data in Table 1 that the anti-aging non-crystalline copolyester materials in Examples 1-3 of the present invention have the advantages of good mechanical properties, corrosion resistance, aging resistance and high transparency. From the comparison between Example 4 and Example 1, it can be seen that changing the ratio of the polymerizable ultraviolet absorber will cause part of the polymerizable ultraviolet absorber to remain in the system, thereby reducing the mechanical properties and corrosion resistance of the copolyester material; from the comparison between Example 5 and Example 1, it can be seen that changing the ratio of terephthalic acid containing ultraviolet light absorbing segments and introducing ultraviolet absorbing segments into the copolyester segments will increase the rigidity of the copolyester molecular chain, thereby reducing the impact strength and the corrosion resistance of the copolyester; from the comparison between Example 6 and Example 1, it can be seen that changing the ratio of terephthalic acid containing ultraviolet light absorbing segments and introducing ultraviolet absorbing segments into the copolyester segments will increase the rigidity of the copolyester molecular chain, thereby reducing the impact strength and the corrosion resistance of the copolyester; 1, it can be seen that the mechanical properties, corrosion resistance and aging resistance of the copolyester material are further improved after the modified glass flakes are added; from the comparison of Examples 7 and 8 with Example 6, it can be seen that the changed ratio of isocyanate or activated glass flakes will make the residual -NCO groups in the system insufficient to produce the effect of promoting the crosslinking formed inside the copolyester, thereby reducing the mechanical properties of the copolyester; from the comparison of Example 9 and Example 6, it can be seen that only adding glass flakes, the compatibility of glass flakes with copolyester is poor, which reduces the various properties of the copolyester; from the comparison of Comparative Example 1 and Example 1, it can be seen that adding unmodified PETG, the mechanical properties and aging resistance of the copolyester are poor and the transparency is low.
[0126] The above implementation modes are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. An anti-aging non-crystalline copolyester material, characterized in that: The invention comprises the following raw materials in parts by weight: 30-50 parts of modified PETG, 10-15 parts of filler, 3-5 parts of flame retardant and 0.5-1 part of antioxidant.
2. The anti-aging non-crystalline copolyester material according to claim 1, characterized in that: The preparation method of the modified PETG comprises the following steps: A1. Add 2-hydroxyterephthalic acid, acrylic acid and tetraisopropyl titanate into a reaction vessel, and react at 70-80° C. for 1-2 hours to obtain terephthalic acid containing a double bond; A2, adding the double-bond-containing terephthalic acid obtained in step A1, a polymeric ultraviolet light absorber and dibenzoyl peroxide into a reaction vessel, and reacting at 80-90° C. for 2-4 hours to obtain terephthalic acid containing ultraviolet light absorbing segments; A3. Add terephthalic acid containing ultraviolet light absorbing segments obtained in step A2, terephthalic acid, ethylene glycol, 1,4-cyclohexanedimethanol, neopentyl glycol and germanium dioxide into a reaction vessel, heat to 240-260° C., react at 0.2-0.3 MPa, adjust the pressure to 95-105 Pa when the water output reaches 99.3-99.7% of the theoretical water output value, heat to 270-290° C., react for 2-3 hours, and obtain modified PETG.
3. The anti-aging non-crystalline copolyester material according to claim 2, characterized in that: The polymeric ultraviolet absorber is 2-hydroxy-4-methacryloxybenzophenone or 2-hydroxy-4-allyloxybenzophenone.
4. The anti-aging non-crystalline copolyester material according to claim 2, characterized in that: The mass ratio of the double-bond-containing terephthalic acid to the polymeric ultraviolet absorber in step A2 is 1:(0.7-0.9).
5. The anti-aging non-crystalline copolyester material according to claim 2, characterized in that: The mass ratio of ethylene glycol, terephthalic acid, terephthalic acid containing ultraviolet light absorbing segments, 1,4-cyclohexanedimethanol and neopentyl glycol in step A3 is (1.3-1.6):(2.4-2.7):(0.5-0.7):0.5:0.
5.
6. The anti-aging non-crystalline copolyester material according to claim 1, characterized in that: The anti-aging non-crystalline copolyester material also contains 5-7 parts by weight of modified glass flakes.
7. The anti-aging non-crystalline copolyester material according to claim 6, characterized in that: The method for preparing the modified glass flakes comprises the following steps: B1. Add glass flakes and N,N-dimethylformamide to a reaction vessel, perform ultrasonication for 30-60 minutes, add isocyanate, stir at 60-70° C. for 2-4 hours, cool to room temperature, wash with anhydrous ethanol for 3-5 times, filter, and dry to obtain activated glass flakes; B2. Add the activated glass flakes obtained in step B1, N,N-dimethylformamide and 2-hydroxy-4-(2,3-epoxypropoxy)benzophenone into a reaction vessel, heat to 60-70°C, and stir for 2-3 hours to obtain modified glass flakes.
8. The anti-aging non-crystalline copolyester material according to claim 7, characterized in that: The mass ratio of the glass flakes to the isocyanate in step B1 is (1-3):
1.
9. The anti-aging non-crystalline copolyester material according to claim 7, characterized in that: The mass ratio of the activated glass flakes and 2-hydroxy-4-(2,3-epoxypropoxy)benzophenone in step B2 is (2-4):
1.
10. A method for preparing the anti-aging non-crystalline copolyester material according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1. Mix the modified PETG, filler, flame retardant and antioxidant, add them into a mixer, and mix for 10-30 minutes to obtain a premix; S2. The premix obtained in step S1 is put into a twin-screw extruder, extruded from a die head, and pelletized. The extrusion temperature is controlled at 210-220° C. to obtain an anti-aging non-crystalline copolyester material.
Citation Information
Cited By
Matt PETG polyester material and preparation method thereof
CN122060296A