High-molecular polymer material with electromagnetic interference resistance and preparation method thereof
By using polymer polymers, enhanced modified materials and electromagnetic shielding modified materials in anti-electromagnetic interference polymer materials, and combining pore-generating agents to form microporous structures, the problems of high material cost, increased density and insufficient conductivity are solved. , achieving more efficient electromagnetic shielding effect.
Patent Information
- Application Number
- CN202411214599.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-01
- Publication Date
- 2024-11-12
AI Technical Summary
The existing electromagnetic interference-resistant polymer materials have high production costs, increased density and insufficient conductivity, which cannot meet the application needs of extremely high conductivity.
Using a combination of polymer polymers, enhanced modified materials, electromagnetic shielding modified materials and pore-generating agents, the microporous composite electromagnetic shielding structure is formed through ultrasonic dissolution and heating, and the expansion microspheres are used to reduce weight and cost and increase Conductivity and electromagnetic shielding effect.
It effectively reduces the weight and production cost of materials, while improving conductivity and electromagnetic shielding performance, and is suitable for applications that require high conductivity.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the field of polymer materials, and in particular to a polymer material with anti-electromagnetic interference function and a preparation method thereof. Background Art
[0002] The existing anti-electromagnetic interference (EMI) polymer material is a high-performance engineering plastic designed specifically to reduce electromagnetic radiation interference in electronic equipment. This material combines excellent electromagnetic shielding performance with ease of processing, providing an ideal protection solution for modern electronic equipment.
[0003] This anti-electromagnetic interference material is composed of a special polymer matrix, conductive fillers and a variety of additives. After precise formula design and manufacturing process, the material has excellent electromagnetic shielding performance while maintaining high mechanical strength. The addition of conductive fillers forms a continuous conductive network inside the material, which can effectively absorb and reflect electromagnetic waves, thereby significantly reducing the leakage and interference of electromagnetic radiation.
[0004] During the molding process, the material exhibits excellent fluidity and moldability, and can easily adapt to various complex mold structures to achieve high-precision and high-efficiency production. At the same time, the material also has good thermal and chemical stability, and can maintain stable performance in various harsh environments.
[0005] In addition, anti-electromagnetic interference materials also have excellent electrical insulation and wear resistance, which can effectively protect electronic equipment from damage caused by electrical short circuits and mechanical wear. These performance characteristics make this material have broad application prospects in the fields of communications, medical treatment, aerospace, etc.
[0006] Although existing anti-electromagnetic interference (EMI) materials have many advantages, they still have some potential disadvantages in practical applications:
[0007] Higher cost: Because anti-electromagnetic interference materials contain special conductive fillers and additives, their production costs are usually higher than ordinary materials.
[0008] Increased weight: In order to obtain a good electromagnetic shielding effect, anti-electromagnetic interference materials need to add a large amount of conductive fillers, which may lead to an increase in the density of the material, making the finished product heavier.
[0009] Electrical conductivity limitations: Although EMI-resistant materials have some electrical conductivity, they are generally not as conductive as metals or other highly conductive materials; therefore, they are not suitable for applications that require extremely high electrical conductivity. Summary of the invention
[0010] The main purpose of the present invention is to provide a high molecular polymer material with anti-electromagnetic interference and a preparation method thereof.
[0011] To achieve the above object, the technical solution adopted by the present invention is:
[0012] A high molecular polymer material with anti-electromagnetic interference properties. The raw material components, based on the total mass of the raw materials being 100, include 40-65 parts by weight of high molecular polymer, 10-20 parts by weight of enhanced modified material, 10-20 parts by weight of electromagnetic shielding modified material, 5-10 parts by weight of solvent and 5-10 parts by weight of porogen.
[0013] Furthermore, the high molecular polymer is a combination of one or more of polyamide 6, polyamide 66, polyamide 610, and polybutylene terephthalate.
[0014] Furthermore, the reinforcing modified material is a combination of one or more of carbon fiber, glass fiber and mineral fiber.
[0015] Furthermore, the electromagnetic shielding modified material is a combination of one or more of reduced graphene oxide, conductive carbon black, conductive graphite, and carbon nanotubes.
[0016] Furthermore, the porogen is an expandable microsphere, and the expandable microsphere includes an outer shell and an inner filler.
[0017] Furthermore, the outer shell is an expandable outer shell made of a polymer material, and the inner filler includes a liquid or solid that is volatile when heated.
[0018] Furthermore, the method for preparing the raw material comprises the steps of
[0019] S1: dispersing and mixing, mixing the solvent and the electromagnetic shielding modified material with a total mass of 100, so that the electromagnetic shielding modified material is dissolved and dispersed in the solvent by ultrasound to form a uniform mixture;
[0020] S2 is initially fused, the polymer is softened by heating, and the reinforcing modified material and the mixture obtained in S1 are fully mixed with the polymer;
[0021] S3: adding the porogen, after the polymer mixture is mixed, quickly adding the porogen and stirring quickly and evenly to make it uniformly dispersed in the polymer mixture, and quickly cooling the polymer mixture with the porogen added;
[0022] S4 forming, pelletizing or cutting the cooled product.
[0023] Furthermore, in step S3, the porogen is mixed with the room temperature powder of the polymer before being added to the molten polymer mixture, and then added to the fusion of the polymer together.
[0024] Furthermore, an anti-electromagnetic interference product is prepared by heating and melting the raw materials.
[0025] Furthermore, the product forms a high molecular polymer microporous composite electromagnetic shielding structure through a porogen, a reinforcing modified material and an electromagnetic shielding modified material.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] The present invention adds expandable microspheres to form pores inside the raw materials during product production due to the expansion of the expandable microspheres, thereby reducing the overall weight of the product, saving preparation raw materials, and reducing production costs;
[0028] Electromagnetic shielding modified materials are also added to the raw materials. The electromagnetic shielding modified materials give the product a certain conductivity, making it anti-electromagnetic interference. At the same time, the electromagnetic shielding modified materials are combined with the pores of expandable microspheres, so that the pores can better reflect electromagnetic signals, thus improving the anti-electromagnetic effect.
[0029] The addition of enhanced modified materials can improve the stability of the overall structure of the product, while reducing the weight of the product and reducing the disadvantages of structural deterioration caused by pores generated by the expansion of expandable microspheres. DETAILED DESCRIPTION
[0030] The preferred embodiments of the present invention are described in detail below so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby making a clearer and more definite definition of the protection scope of the present invention.
[0031] Example 1
[0032] Preparation of high molecular polymer material with anti-electromagnetic interference, based on the total mass of raw materials as 100, prepare 65 weight parts of high molecular polymer, 10 weight parts of enhanced modified material, 10 weight parts of electromagnetic shielding modified material, 5 weight parts of solvent and 10 weight parts of porogen.
[0033] The high molecular polymer is polyamide 6, the reinforced modified material is carbon fiber, the electromagnetic shielding modified material is reduced graphene oxide, the porogen is expandable microspheres, and the solvent is an ester solvent.
[0034] Mixing the solvent and the electromagnetic shielding modified material in an amount of 100 grams in total weight, so that the electromagnetic shielding modified material is dissolved and dispersed in the solvent by ultrasound to form a uniform mixture;
[0035] The high molecular polymer is softened by heating, and the reinforcing modified material and the obtained mixture are thoroughly mixed with the high molecular polymer;
[0036] After the polymer mixture is mixed, the porogen is quickly added and stirred to be uniformly dispersed in the polymer mixture, and the porogen is quickly added to the polymer mixture and cooled;
[0037] Finally, the cooled raw materials are pelletized and the pore-forming agent morphology inside the raw materials is detected.
[0038] Example 2
[0039] The preparation scheme of this embodiment is the same as that of Example 1, and the difference is that: based on the total mass of raw materials as 100, there are 40 weight parts of high molecular polymer, 20 weight parts of reinforcing modified material, 20 weight parts of electromagnetic shielding modified material, 10 weight parts of solvent and 10 weight parts of porogen.
[0040] Finally, the cooled raw materials are pelletized and the pore-forming agent morphology inside the raw materials is detected.
[0041] Example 3
[0042] The preparation scheme of this embodiment is the same as that of Embodiment 1-2, and the difference is that: based on the total mass of raw materials as 100, there are 50 weight parts of high molecular polymer, 20 weight parts of reinforcing modified material, 15 weight parts of electromagnetic shielding modified material, 10 weight parts of solvent and 5 weight parts of porogen.
[0043] Finally, the cooled raw materials are pelletized and the pore-forming agent morphology inside the raw materials is detected.
[0044] Example 4
[0045] The preparation scheme of this embodiment is the same as that of Embodiment 1, except that the polymer is divided into two parts, one for preparing the polymer mixture, and the other for: before adding the porogen to the molten polymer mixture, the porogen is first mixed with the polymer room temperature powder and added together to the polymer fusion.
[0046] Finally, the cooled raw materials are pelletized and the pore-forming agent morphology inside the raw materials is detected.
[0047] Expansion rate of the raw material internal porogen prepared in the example:
[0048] Product Name Porogenic agent expansion rate % Example 1 19 Example 2 16 Example 3 17 Example 4 8
[0049] Experimental Example 1
[0050] The raw material prepared in Example 1 is used to form an anti-electromagnetic interference product.
[0051] Experimental Example 2
[0052] The raw material prepared in Example 2 is used to form an anti-electromagnetic interference product.
[0053] Experimental Example 3
[0054] The raw material prepared in Example 3 is used to form an anti-electromagnetic interference product.
[0055] Experimental Example 4
[0056] The raw material prepared in Example 4 is used to prepare a molded anti-electromagnetic interference product.
[0057] The thickness of the prepared products is 1.5 mm.
[0058] The test performance data of the products made in Experimental Examples 1-4 are as follows:
[0059]
[0060] Comprehensive test data show that the electromagnetic shielding performance of Experimental Example 4 is the best and the density is lower. It can be seen that the smaller the expansion rate of the expandable microspheres when they are made into raw materials, the better the electromagnetic shielding performance of the manufactured product and the lower the density.
[0061] It should be noted that the high molecular polymer is a combination of one or more of polyamide 6, polyamide 66, polyamide 610 and polybutylene terephthalate.
[0062] The reinforcing modified material is a combination of one or more of carbon fiber, glass fiber and mineral fiber.
[0063] The electromagnetic shielding modified material is a combination of one or more of reduced graphene oxide, conductive carbon black, conductive graphite and carbon nanotubes.
[0064] The porogen is expandable microspheres, which include an outer shell and an inner filler.
[0065] The outer shell is an expandable shell made of a polymer material, and the inner filler comprises a liquid or solid that is easily volatile when heated.
[0066] The above description is only a preferred embodiment of the present invention, and the protection scope of the present invention is not limited to the above embodiment. Any equivalent modifications or changes made by ordinary technicians in this field based on the contents disclosed by the present invention should be included in the protection scope recorded in the claims.
Claims
1. A polymer material with anti-electromagnetic interference, characterized in that: The raw material components, based on the total mass of the raw materials being 100, include 40-65 parts by weight of high molecular polymer, 10-20 parts by weight of enhanced modified material, 10-20 parts by weight of electromagnetic shielding modified material, 5-10 parts by weight of solvent and 5-10 parts by weight of porogen.
2. The high molecular polymer material with anti-electromagnetic interference according to claim 1, characterized in that: The high molecular polymer is a combination of one or more of polyamide 6, polyamide 66, polyamide 610 and polybutylene terephthalate.
3. The high molecular polymer material with anti-electromagnetic interference according to claim 1, characterized in that: The reinforcing modified material is a combination of one or more of carbon fiber, glass fiber and mineral fiber.
4. The high molecular polymer material with anti-electromagnetic interference according to claim 1, characterized in that: The electromagnetic shielding modified material is a combination of one or more of reduced graphene oxide, conductive carbon black, conductive graphite and carbon nanotubes.
5. The high molecular polymer material with anti-electromagnetic interference according to claim 1, characterized in that: The porogen is expandable microspheres, which include an outer shell and an inner filler.
6. The high molecular polymer material with anti-electromagnetic interference according to claim 5, characterized in that: The outer shell is an expandable shell made of a polymer material, and the inner filler comprises a liquid or solid that is easily volatile when heated.
7. A method for preparing the raw material according to any one of claims 1 to 6, characterized in that , including the steps S1: dispersing and mixing, mixing the solvent and the electromagnetic shielding modified material with a total mass of 100, so that the electromagnetic shielding modified material is dissolved and dispersed in the solvent by ultrasound to form a uniform mixture; S2 is initially fused, the polymer is softened by heating, and the reinforcing modified material and the mixture obtained in S1 are fully mixed with the polymer; S3: adding the porogen, after the polymer mixture is mixed, quickly adding the porogen and stirring quickly and evenly to make it uniformly dispersed in the polymer mixture, and quickly cooling the polymer mixture with the porogen added; S4 forming, pelletizing or cutting the cooled product.
8. The method for preparing the raw material according to claim 7, characterized in that: In step S3, the porogen is mixed with the room temperature powder of the polymer before being added to the molten polymer mixture, and then added to the fusion of the polymer together.
9. A product that resists electromagnetic interference, characterized in that: A product prepared by heating and melting the raw material as claimed in any one of claims 1 to 6.
10. The anti-electromagnetic interference product according to claim 9, characterized in that: The product forms a high molecular polymer microporous composite electromagnetic shielding structure through a porogen, a reinforcing modified material and an electromagnetic shielding modified material.