Nylon hook for glass fiber twisting and preparation method thereof
By mixing cellulose powder and lignin with nylon matrix and other materials after special pretreatment, a nylon hook for glass fiber twisted wire with stronger wear resistance and higher strength was prepared, which solved the problem of attenuation of existing nylon hooks. , improves the quality and efficiency of glass fiber production.
Patent Information
- Application Number
- CN202411222604.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-12
AI Technical Summary
The existing nylon hooks for glass fiber twisted wires are fast attenuated under the guidance of long-term and high-speed glass fibers, resulting in high defect rate of glass fiber hairs and unstable equipment operation, making it difficult to improve production efficiency.
A preparation method is adopted to prepare lignin-cellulose-based carbon fibers by mixing cellulose powder and lignin after special pretreatment, and mixing them with nylon matrix, graphite and additives in a specific ratio to bake , extrusion and molding of injection molding machine to produce nylon hooks for glass fiber twisted wires with stronger wear resistance and higher strength.
It significantly reduces the hair loss rate, head break rate and uneven rate in the production process of glass fiber, improves production quality and efficiency, has a higher applicable speed, and a shorter replacement cycle, reducing production costs.
Smart Images

Figure CN118931171A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of glass fibers, and in particular to a nylon hook for glass fiber twisting and a preparation method thereof. Background Art
[0002] At present, most nylon hooks used for glass fiber twisting have a hook body on the top and a hook body on the bottom. The fibers pass through the hook body of the nylon hook to twist the yarn. In the twisting equipment, the nylon hook is a key component for yarn guidance, and its material properties directly affect the transmission quality of the glass fiber and the operating efficiency of the equipment. Although traditional nylon hooks have basic wear resistance and strength, their performance decays rapidly under long-term, high-speed glass fiber guidance, making it difficult to meet the high performance requirements of glass fiber twisting equipment for nylon hooks, which easily leads to a high glass fiber hairiness defect rate. In addition, the twisting equipment runs too fast, which can easily cause the nylon hook to break, thereby failing to improve production efficiency.
[0003] Currently, the nylon hook for glass fiber twisting, which is the most widely used, most efficient and has the lowest hairiness defect rate in this field, comes from Carter Company in the United States. Therefore, it is of great significance to overcome the problem of high hairiness defect rate of glass fiber caused by nylon hooks in the existing glass fiber production process and provide a nylon hook for glass fiber twisting that can improve both the quality and efficiency of glass fiber production. Summary of the invention
[0004] The purpose of the invention is to overcome the problem of low production quality and production efficiency of glass fiber caused by nylon hooks in the existing glass fiber production process.
[0005] In order to achieve the above object, the first aspect of the present invention provides a method for preparing a nylon hook for glass fiber twisting yarn, comprising the following steps:
[0006] The components in the raw material composition are mixed and then subjected to baking treatment, injection molding machine extrusion treatment and molding treatment in sequence to obtain the nylon hook for glass fiber twisting wire;
[0007] The raw material composition comprises 75wt%-90wt% of a nylon matrix, 5wt%-10wt% of a lignin-cellulose-based carbon fiber, 3wt%-10wt% of graphite and 0.1wt%-7wt% of an additive;
[0008] The lignin-cellulose based carbon fiber is prepared by the following method:
[0009] S1: dispersing cellulose powder in a ZnCl2 solution and performing a first solvent removal treatment to obtain modified cellulose powder;
[0010] and, dispersing lignin in acetone to obtain a lignin suspension;
[0011] S2: immersing the modified cellulose powder in the lignin suspension, and then performing a second solvent removal treatment to obtain a lignin-cellulose matrix;
[0012] S3: subjecting the lignin-cellulose matrix to melt spinning, pre-oxidation and carbonization treatments in sequence to obtain lignin-cellulose based carbon fibers.
[0013] The second aspect of the present invention provides a nylon hook for glass fiber twisting yarn produced by the above-mentioned preparation method.
[0014] The preparation method of the nylon hook for glass fiber twisting provided by the present invention is conducive to mixing cellulose powder and lignin after special pretreatment to obtain lignin-cellulose based carbon fiber. Compared with conventional carbon fiber, the lignin-cellulose based carbon fiber has higher strength and better toughness. When added to a raw material composition with a specific ratio, the lignin-cellulose based carbon fiber has better compatibility with other components in the raw material composition, and synergistically enhances the effect. The prepared nylon hook for glass fiber twisting can greatly reduce the hairiness defect rate, breakage rate and unevenness rate in the glass fiber production process, and can greatly improve the production quality of glass fiber. In addition, the nylon hook for glass fiber twisting provided by the present invention has a higher applicable rotation speed and a shorter replacement cycle, which greatly improves the production efficiency of glass fiber. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is a physical picture of the nylon hook provided in Example 1 of the present invention after continuous production of glass fiber for 48 hours;
[0016] Figure 2 This is a physical picture of the nylon hook provided for Comparative Example 5 after 48 hours of continuous production of glass fiber. DETAILED DESCRIPTION
[0017] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0018] As mentioned above, the first aspect of the present invention provides a method for preparing a nylon hook, the method comprising the following steps:
[0019] The components in the raw material composition are mixed and then subjected to baking treatment, injection molding machine extrusion treatment and molding treatment in sequence to obtain the nylon hook for glass fiber twisting wire;
[0020] The raw material composition comprises 75wt%-90wt% of a nylon matrix, 5wt%-10wt% of a lignin-cellulose-based carbon fiber, 3wt%-10wt% of graphite and 0.1wt%-7wt% of an additive;
[0021] The lignin-cellulose based carbon fiber is prepared by the following method:
[0022] S1: dispersing cellulose powder in a ZnCl2 solution and performing a first solvent removal treatment to obtain modified cellulose powder;
[0023] and, dispersing lignin in acetone to obtain a lignin suspension;
[0024] S2: immersing the modified cellulose powder in the lignin suspension, and then performing a second solvent removal treatment to obtain a lignin-cellulose matrix;
[0025] S3: subjecting the lignin-cellulose matrix to melt spinning, pre-oxidation and carbonization treatments in sequence to obtain lignin-cellulose based carbon fibers.
[0026] The preparation method of the nylon hook for glass fiber twisting provided by the present invention utilizes cellulose powder and lignin to be specially pretreated and then mixed to obtain lignin-cellulose-based carbon fiber. Compared with conventional carbon fiber, the lignin-cellulose-based carbon fiber has higher strength and better toughness. When added to a raw material composition with a specific ratio, the lignin-cellulose-based carbon fiber has better compatibility with other components in the raw material composition, and synergistically enhances the effect. The prepared nylon hook has stronger wear resistance and higher strength, and better stability in practical applications. It can not only greatly reduce the hairiness defect rate, breakage rate and unevenness rate in the glass fiber production process, but also can be operated in a glass fiber twisting machine with a higher operating speed, thereby greatly improving the production efficiency of the glass fiber.
[0027] Furthermore, from the perspective of production and application, lignin and cellulose are inexpensive, the preparation steps of the nylon hooks for glass fiber twisted yarn provided by the present invention are simple, no polishing or grinding is required after the molding process, the production cost is low, and it can be put into mass production.
[0028] According to some preferred embodiments of the present invention, in step S1, the concentration of the ZnCl2 solution is 0.1 g / ml-0.5 g / ml, and the usage ratio of the cellulose powder to the ZnCl2 solution is 3 mg / ml-5 mg / ml. Under this preferred condition, the obtained nylon hook for glass fiber twisting has lower hairiness defect rate, broken end rate and unevenness rate in the process of producing glass fiber.
[0029] It should be noted that the dosage ratio of the cellulose powder to the ZnCl2 solution is 3 mg / ml-5 mg / ml, which means that the dosage of the cellulose powder is 3 mg-5 mg for every 1 ml of the ZnCl2 solution.
[0030] Particularly preferably, the particle size d50 of the cellulose powder is 180 μm-280 μm.
[0031] Particularly preferably, the pH value of the ZnCl2 solution is 6-6.5. Exemplarily, the pH value of the ZnCl2 solution is adjusted by adding dilute hydrochloric acid. Under this preferred condition, the nylon hook for glass fiber twisting wire has better performance. The inventors of the present invention speculate that in a slightly acidic environment, the cellulose powder reacts with the Zn in the ZnCl2 solution. 2+ The lignin-cellulose-based carbon fibers can be better combined, thereby enhancing the performance of the prepared lignin-cellulose-based carbon fibers, so that the lignin-cellulose-based carbon fibers can produce better synergistic effects with other components in the raw material composition, further enhancing various aspects of the performance of the nylon hooks, and improving the production efficiency and production quality of the glass fibers.
[0032] According to some preferred embodiments of the present invention, in step S1, the cellulose powder is dispersed in the ZnCl2 solution by a first ultrasonic treatment, the power of the first ultrasonic treatment is 800W-1000W, and the treatment time is 3h-5h.
[0033] According to some preferred embodiments of the present invention, in step S1, the first solvent removal process comprises a filtration process and a washing process performed in sequence. Exemplarily, the washing process is performed using an ethanol aqueous solution with a concentration of 50 vol%-70 vol%, and the number of washing processes is 2-5 times.
[0034] According to some preferred embodiments of the present invention, in step S1, the dosage ratio of the lignin to the acetone is 40 mg / ml-60 mg / ml. It should be noted that the dosage ratio of the lignin to the acetone is 40 mg / ml-60 mg / ml, which means that the dosage of the lignin is 40 mg-60 mg for every 1 ml of acetone.
[0035] According to some preferred embodiments of the present invention, in step S1, the lignin is dispersed in the acetone by a second ultrasonic treatment, the power of the second ultrasonic treatment is 600W-800W, and the treatment time is 1h-3h.
[0036] According to some preferred embodiments of the present invention, in step S2, the modified cellulose powder subjected to the immersion treatment is used in an amount ratio of 1:1 to 1.5 to the lignin suspension. Under this preferred condition, the obtained nylon hook for glass fiber twisting has lower hairiness defect rate, broken end rate and unevenness rate in the process of producing glass fiber.
[0037] According to some preferred embodiments of the present invention, in step S2, the immersion time of the immersion treatment is 30 min-60 min. Particularly preferably, the immersion treatment is accompanied by at least one of stirring treatment and ultrasonic dispersion treatment.
[0038] According to some preferred embodiments of the present invention, in step S2, the second solvent removal process comprises a filtration process and a washing process performed in sequence. Exemplarily, the washing process is performed using an ethanol aqueous solution with a concentration of 50 vol%-70 vol%, and the number of washing processes is 2-5 times.
[0039] According to some preferred embodiments of the present invention, in step S3, the spinning temperature of the melt spinning process is 160°C-260°C, and the spinning speed is 600m / min-800m / min. It should be noted that the spinning speed is 600m / min-800m / min, which means that 600m-800m is spun per minute.
[0040] According to some preferred embodiments of the present invention, in step S3, the pre-oxidation treatment is carried out in the following manner: in air, the raw silk obtained by the melt spinning treatment is heated to 200°C-300°C at a heating rate of 2°C / min-4°C / min, and kept at a constant temperature for 30min-60min to obtain pre-oxidized silk.
[0041] According to some preferred embodiments of the present invention, in step S3, the carbonization treatment is carried out in the following manner: in a protective gas, the pre-oxidized fiber is heated to 1000°C-1400°C at a heating rate of 4°C / min-6°C / min, and the temperature is kept constant for 1h-2h to obtain lignin-cellulose based carbon fiber.
[0042] It should be noted that the protective gas is one or more of nitrogen and inert gas. In a particularly preferred embodiment of the present invention, the protective gas is nitrogen.
[0043] According to some preferred embodiments of the present invention, the nylon matrix comprises at least one of nylon 6 and nylon 66.
[0044] Particularly preferably, the molding temperature of the nylon matrix is 230°C-300°C, and the density is 1.14 g / cm 3-1.15g / cm 3 , the flexural strength is 60MPa-110MPa.
[0045] According to some preferred embodiments of the present invention, the auxiliary agent comprises at least one of a heat stabilizer, a light stabilizer and a plasticizer.
[0046] It should be noted that the present invention has no special requirements on the types of materials of the heat stabilizer, light stabilizer and plasticizer, and the materials conventionally used in the art may be used.
[0047] Further preferably, in the raw material composition, the amount of the heat stabilizer is 3wt%-5wt%, the amount of the light stabilizer is 0.5wt%-1wt%, and the amount of the plasticizer is 0.3wt%-1wt%.
[0048] According to some preferred embodiments of the present invention, the baking temperature is 130° C.-190° C., and the baking time is 1 h-4 h.
[0049] According to some preferred embodiments of the present invention, the temperature of the extrusion process of the injection molding machine is 350°C-450°C.
[0050] According to some preferred embodiments of the present invention, the molding process is carried out in a mold, the temperature of the mold is 150° C.-200° C., and the mold is naturally cooled until the nylon hook is solidified and molded.
[0051] The second aspect of the present invention provides a nylon hook for glass fiber twisting yarn produced by the aforementioned preparation method.
[0052] The nylon hook provided by the present invention has stronger wear resistance and higher strength, better stability in practical applications, and can greatly reduce the hairiness defect rate in the glass fiber production process.
[0053] The present invention will be described in detail below by way of examples. The present invention will be described in detail below by way of examples. In the following examples, unless otherwise specified, the raw materials used are all common commercially available products.
[0054] Nylon 6: purchased from Huaguang (Shanghai) Plastics Co., Ltd.;
[0055] Graphite: Graphite powder, purchased from Qingdao Kaiyueda New Energy Materials Co., Ltd., item number 01;
[0056] Heat stabilizer: purchased from Chongqing Baohua Chemical Additive Factory, specification is XJ-169 series;
[0057] Light stabilizer: purchased from Dongguan Shanyi Plastic Co., Ltd., brand name UV-770;
[0058] Plasticizer: purchased from Shandong Huayao Biotechnology Co., Ltd., brand name TXIB;
[0059] Cellulose powder: purchased from Shanghai MacLean Biochemical Technology Co., Ltd., brand C823054, d50 180-280 μm;
[0060] Lignin: purchased from Wuhan Lanabai Pharmaceutical Chemical Co., Ltd., brand number 9005-53-2, analytical grade AR;
[0061] Conventional carbon fiber: purchased from Jiangxi Shuobang New Material Technology Co., Ltd., carbon fiber powder 30-500 mesh.
[0062] The model of the nylon hooks prepared in the following examples is E-25-CM ISO 162-170.
[0063] Example 1
[0064] The components in the raw material composition are mixed and then sequentially subjected to baking treatment, injection molding machine extrusion treatment and molding treatment to obtain a nylon hook G1 for glass fiber twisting;
[0065] The baking treatment is carried out at a temperature of 160°C for 3 hours. The injection molding extrusion treatment is carried out in an injection molding machine at a temperature of 400°C. The molding treatment is carried out in a mold at a temperature of 180°C.
[0066] The specific ratio of the raw material composition is: 80.8wt% of nylon 6, 6wt% of lignin-cellulose based carbon fiber L1, 8wt% of graphite, 4wt% of heat stabilizer, and 0.8wt% of light stabilizer.
[0067] 0.4wt% plasticizer
[0068] Lignin-cellulose based carbon fiber L1 was prepared by the following method:
[0069] S1: dispersing cellulose powder in a ZnCl2 solution and performing a first solvent removal treatment to obtain modified cellulose powder; the first solvent removal treatment comprises a filtration treatment and a washing treatment performed in sequence, the filter membrane of the filtration treatment is 45 μm, and the washing treatment is performed using a 50 vol% ethanol aqueous solution, and the washing is repeated 3 times;
[0070] and, dispersing lignin in acetone to obtain a lignin suspension;
[0071] S2: After the modified cellulose powder is immersed in the lignin suspension, a second solvent removal treatment is performed to obtain a lignin-cellulose matrix; the second solvent removal treatment comprises a filtration treatment and a washing treatment performed in sequence, the filter membrane of the filtration treatment is 45 μm, and the washing treatment is performed using a 50 vol% ethanol aqueous solution, and the washing is repeated 3 times;
[0072] S3: subjecting the lignin-cellulose matrix to melt spinning, preoxidation and carbonization treatments in sequence to obtain lignin-cellulose based carbon fibers;
[0073] The parameters of steps S1-S3 are shown in Table 1 below.
[0074] Embodiment 2-5
[0075] The method of Example 1 was followed, except that some parameters in the preparation process of lignin-cellulose-based carbon fiber were adjusted, as shown in Table 1 below. The remaining step parameters were the same as those of Example 1, and nylon hooks G2-G5 for glass fiber twisting were prepared respectively.
[0076] Comparative Example 1
[0077] Cellulose powder and lignin in a mass ratio of 1:1.2 were mixed and melt-spinning, pre-oxidation and carbonization were performed in sequence to obtain lignin-cellulose based carbon fiber DL1.
[0078] Among them, the control parameters of the melt spinning treatment, pre-oxidation treatment and carbonization treatment are the same as those in Example 1.
[0079] The lignin-cellulose-based carbon fiber L1 in the raw material composition in Example 1 is replaced with the lignin-cellulose-based carbon fiber DL1, and then the components in the raw material composition are mixed and sequentially subjected to baking treatment, injection molding machine extrusion treatment and molding treatment to obtain a nylon hook DG1 for glass fiber twisting;
[0080] Among them, the control parameters of the baking process, the injection molding machine extrusion process and the molding process are the same as those in Example 1.
[0081] Comparative Example 2
[0082] The lignin is subjected to melt spinning, pre-oxidation and carbonization to obtain the lignin-based carbon fiber DL2.
[0083] Among them, the control parameters of the melt spinning treatment, pre-oxidation treatment and carbonization treatment are the same as those in Example 1.
[0084] The lignin-cellulose-based carbon fiber L1 in the raw material composition in Example 1 is replaced with the lignin-cellulose-based carbon fiber DL2, and then the components in the raw material composition are mixed and sequentially subjected to baking treatment, injection molding machine extrusion treatment and molding treatment to obtain a nylon hook DG2 for glass fiber twisting;
[0085] Among them, the control parameters of the baking process, the injection molding machine extrusion process and the molding process are the same as those in Example 1.
[0086] Comparative Example 3
[0087] The cellulose powder is subjected to melt spinning, pre-oxidation and carbonization to obtain the cellulose-based carbon fiber DL3.
[0088] Among them, the control parameters of the melt spinning treatment, pre-oxidation treatment and carbonization treatment are the same as those in Example 1.
[0089] The lignin-cellulose-based carbon fiber L1 in the raw material composition in Example 1 is replaced with the lignin-cellulose-based carbon fiber DL3, and then the components in the raw material composition are mixed and sequentially subjected to baking treatment, injection molding machine extrusion treatment and molding treatment to obtain a nylon hook DG3 for glass fiber twisting;
[0090] Among them, the control parameters of the baking process, the injection molding machine extrusion process and the molding process are the same as those in Example 1.
[0091] Comparative Example 4
[0092] The lignin-cellulose-based carbon fiber L1 in the raw material composition in Example 1 is replaced with a conventional carbon fiber, and then the components in the raw material composition are mixed and sequentially subjected to baking treatment, injection molding machine extrusion treatment and molding treatment to obtain a nylon hook DG4 for glass fiber twisting;
[0093] Among them, the control parameters of the baking process, the injection molding machine extrusion process and the molding process are the same as those in Example 1.
[0094] Comparative Example 5
[0095] The nylon hook DG5 was purchased from Carter Company in the United States, model E-25-CM ISO 162-170.
[0096] Table 1
[0097]
[0098] Test Example: The nylon hooks prepared in the above embodiments and comparative examples were respectively installed and fixed on a glass fiber twisting machine to produce glass fiber twisting. The production was continued for 90 days, and the test results were recorded as shown in Table 2 below.
[0099] Table 2
[0100] G1 G2 G3 G4 G5 DG1 DG2 DG3 DG4 DG5 Applicable speed (r / min) 6800 6800 6800 6000 6000 5000 4000 4000 4000 4000 24h wear amount / mg 0.52 0.5 0.53 0.68 0.59 1.02 1.33 1.35 1.5 1.31 Replacement cycle / h 72 72 72 72 72 72 48 48 48 48 Glass fiber breakage rate / % 2.23 2.45 2.33 3.87 3.55 4.20 4.96 4.88 5.34 5.10 Glass fiber hairiness defect rate / % 0.80 0.84 0.82 0.97 0.91 1.42 1.87 1.83 2.48 2.35 Uneven rate of glass fiber / % 1.16 1.11 1.23 1.95 1.75 3.57 6.76 6.38 7.45 8.24
[0101] As can be seen from Table 2, the preparation method of the nylon hook provided by the present invention utilizes cellulose powder and lignin to be specially pretreated and then mixed to obtain lignin-cellulose-based carbon fiber, which is added to a raw material composition with a specific ratio. The prepared nylon hook has greatly reduced breakage rate, hairiness defect rate and unevenness rate in glass fiber production, and greatly improved production quality, compared with the nylon hooks of Comparative Examples 1-4 and Carter Company. In addition, the applicable rotation speed of the nylon hook provided by the present invention exceeds 6000r / min, which is much higher than the applicable rotation speed of the nylon hook purchased from Carter Company, and the replacement cycle is also longer, which greatly improves the production efficiency of the glass fiber.
[0102] For example, Figure 1 As shown in the figure, it is a physical picture of the nylon hook made in Example 1 of the present invention after continuous production of glass fiber for 48 hours. Figure 1 As can be seen from the figure, the wear of the nylon hook is very slight, and the wear marks are almost invisible to the naked eye; Figure 2 As shown in the figure, it is a physical picture of the nylon hook purchased from Carter Company in comparative example 5 after continuous production of glass fiber for 48 hours. Figure 2 It can be seen that the nylon hook has obvious signs of wear.
[0103] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing a nylon hook, characterized in that: The following steps are involved: The components in the raw material composition are mixed and then subjected to baking treatment, injection molding machine extrusion treatment and molding treatment in sequence to obtain the nylon hook for glass fiber twisting wire; The raw material composition comprises 75wt%-90wt% of a nylon matrix, 5wt%-10wt% of a lignin-cellulose-based carbon fiber, 3wt%-10wt% of graphite and 0.1wt%-7wt% of an additive; The lignin-cellulose based carbon fiber is prepared by the following method: S1: dispersing cellulose powder in a ZnCl2 solution and performing a first solvent removal treatment to obtain modified cellulose powder; and, dispersing lignin in acetone to obtain a lignin suspension; S2: immersing the modified cellulose powder in the lignin suspension, and then performing a second solvent removal treatment to obtain a lignin-cellulose matrix; S3: subjecting the lignin-cellulose matrix to melt spinning, pre-oxidation and carbonization treatments in sequence to obtain lignin-cellulose based carbon fibers.
2. The preparation method according to claim 1, characterized in that: In step S1, the concentration of the ZnCl2 solution is 0.1 g / ml-0.5 g / ml, and the usage ratio of the cellulose powder to the ZnCl2 solution is 3 mg / ml-5 mg / ml; And / or, in step S1, the cellulose powder is dispersed in the ZnCl2 solution by a first ultrasonic treatment, the power of the first ultrasonic treatment is 800W-1000W, and the treatment time is 3h-5h.
3. The preparation method according to claim 1, characterized in that: In step S1, the dosage ratio of the lignin to the acetone is 40 mg / ml-60 mg / ml; And / or, in step S1, the lignin is dispersed in the acetone by a second ultrasonic treatment, the power of the second ultrasonic treatment is 600W-800W, and the treatment time is 1h-3h.
4. The preparation method according to claim 1, characterized in that: In step S2, the modified cellulose powder and the lignin suspension are used in an amount ratio of 1:1-1.5 for the immersion treatment; And / or, in step S2, the immersion time of the immersion treatment is 30 min-60 min.
5. The preparation method according to any one of claims 1 to 4, characterized in that: In step S1, the particle size d50 of the cellulose powder is 180 μm-280 μm; And / or, in step S1, the pH value of the ZnCl2 solution is 6-6.
5.
6. The preparation method according to any one of claims 1 to 4, characterized in that: In step S3, the spinning temperature of the melt spinning process is 160° C.-260° C., and the spinning speed is 600 m / min-800 m / min; And / or, in step S3, the pre-oxidation treatment is carried out in the following manner: in air, the raw silk obtained by the melt spinning treatment is heated to 200°C-300°C at a heating rate of 2°C / min-4°C / min, and kept at a constant temperature for 30min-60min to obtain pre-oxidized silk; And / or, in step S3, the carbonization treatment is carried out in the following manner: in a protective gas, the pre-oxidized fiber is heated to 1000°C-1400°C at a heating rate of 4°C / min-6°C / min, and kept at a constant temperature for 1h-2h to obtain lignin-cellulose-based carbon fiber.
7. The preparation method according to any one of claims 1 to 4, characterized in that: The nylon matrix comprises at least one of nylon 6 and nylon 66; And / or, the auxiliary agent includes at least one of a heat stabilizer, a light stabilizer, and a plasticizer.
8. The preparation method according to claim 7, characterized in that: The molding temperature of the nylon matrix is 230°C-300°C, and the density is 1.14 g / cm 3 -1.15g / cm 3 , the flexural strength is 60MPa-110MPa.
9. The preparation method according to any one of claims 1 to 4, characterized in that: The baking temperature is 130°C-190°C, and the baking time is 1h-4h; And / or, the extrusion temperature of the injection molding machine is 350°C-450°C; And / or, the molding process is performed in a mold, and the temperature of the mold is 150°C-200°C.
10. Nylon hook for glass fiber twisted yarn obtained by the preparation method according to any one of claims 1 to 9.