High-strength corrosion-resistant polyamide composite material and preparation method thereof
By using polyamide materials with different melting points and modified nanocarbon tubes and other additives, the problem of poor fluidity of polyamide composite materials during the preparation process is solved, the strength and corrosion resistance of the material are improved, and a more efficient preparation process is achieved. .
Patent Information
- Application Number
- CN202411347188.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-11-12
AI Technical Summary
During the preparation process, the existing polyamide composite materials have different melting points and poor fluidity when smelting other materials, which leads to difficult to mix and granulate.
Two polyamide materials with different melting points (polyamide A and polyamide B) are used for melting, and the high melting point polyamide A material maintains fluidity, and add modified carbon nanotubes, heat-resistant agents, and other joints during the melting process. Coupling agents, antioxidants and heat stabilizers can remove impurities through ultrasonic purification and screening, thereby improving the fluidity and strength of the material.
The fluidity and strength of the polyamide composite material is improved, its feasibility during the preparation process is enhanced, and the corrosion resistance and other properties of the material are improved by adding additives.
Smart Images

Figure CN118931179A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyamide composite material preparation, in particular to a high-strength corrosion-resistant polyamide composite material and a preparation method thereof. Background Art
[0002] Polyamide, commonly known as nylon, is a general-purpose engineering plastic with a long history and wide applications. The material has good comprehensive properties, good mechanical properties, heat resistance, chemical resistance, wear resistance, and self-lubricating properties. Polyamide composite materials are typical polymer-based nanocomposites prepared by intercalation polymerization. Clay with a layered structure is also called bentonite, which is a type of non-metallic mineral, and its main component is layered silicates containing montmorillonite. In-situ intercalation polymerization technology is to organicize clay through particle exchange reaction, and then insert polyamide monomers into the lamellar structure of quasi-two-dimensional silicate clay for in-situ polymerization to obtain polymer or clay composite materials. Polyamide composite materials are also widely used in the fields of automobiles, electronics, and machinery.
[0003] However, some deficiencies have emerged in the preparation process of the existing polyamide composite materials, such as the polyamide composite material and its preparation method disclosed in Publication No. CN101875780B. In the preparation process, the polyamide composite material is prepared by using 26-71 parts of nylon 66, 20-40 parts of glass fiber, 10-25 parts of kaolin, 0.1-1 part of antioxidant, 0.2-2 parts of heat stabilizer, 0.1-1 part of lubricant, 0.1-1 part of dispersant and 0.5-2 parts of colorant to produce the polyamide composite material. In the actual production process, since the main material is smelted by nylon 66, in the actual smelting process, the nylon 66 material often has a different melting point from other materials such as glass fiber, which may result in poor fluidity or difficulty in mixing, making it difficult to granulate the polyamide composite material during the manufacturing process.
[0004] Therefore, we propose a high-strength, corrosion-resistant polyamide composite material and a preparation method thereof, in order to solve the problem that during the preparation process of most polyamide composite materials in the existing market mentioned above, since the main material is melted through a nylon material, in the actual melting process, the nylon material often has a different melting point from other materials when melted, which may result in poor fluidity or difficulty in mixing, making it difficult to granulate the polyamide composite material during the manufacturing process. Summary of the invention
[0005] The object of the present invention is to provide a high-strength corrosion-resistant polyamide composite material and a preparation method thereof, so as to solve the problems in the current market raised by the above background technology.
[0006] To achieve the above object, the present invention provides the following technical solution: a high-strength corrosion-resistant polyamide composite material, prepared from the following raw materials in parts by weight:
[0007] Polyamide A: 20-70 parts;
[0008] Polyamide B: 2-30 parts;
[0009] Glass fiber: 10-30 parts;
[0010] Modified carbon nanotubes: 5-15 parts;
[0011] Heat resistant agent: 0.1-1 part;
[0012] Coupling agent: 0.1-1 part;
[0013] Antioxidant: 0.1-1 part;
[0014] Heat stabilizer: 0.5-2 parts;
[0015] Colorant: 0.5-2 parts;
[0016] The melting point of polyamide A is about 20°C higher than that of polyamide B, and the melting point of glass fiber is about 680°C, and the pH of glass fiber is 9-11;
[0017] The preparation method of modified carbon nanotubes is as follows:
[0018] Step 1: Purification
[0019] Place the carbon nanotubes in a container, then pour the decomposition solution into the container, and then use ultrasound to remove impurities such as amorphous carbon and carbon nanoparticles on the carbon nanotube wall. At the same time, the carbon nanotubes will precipitate due to gravity, while impurities such as amorphous carbon and carbon nanoparticles with lower density will float to the top of the solution due to their lower density, thus leaving the surface of the carbon nanotubes.
[0020] Step 2: Mixing
[0021] The purified carbon nanotubes are placed in another container for smelting. When smelting the carbon nanotubes, the temperature needs to reach about 600°C, so that the carbon nanotubes are smelted at high temperature and cracked into carbon atoms. Then, a modification agent is added to reassemble the carbon nanotubes into modified carbon nanotubes. Then, the modified carbon nanotubes are cooled to about 500°C and smelted again.
[0022] Step 3: Cooling
[0023] The modified carbon nanotubes are placed in a cooling box, and the cooling box needs to be maintained at about -10°C so that the modified carbon nanotubes can be cooled quickly; when the modified carbon nanotubes are cooling, ultrasonic equipment can be used to vibrate the inside of the container.
[0024] By using two different polyamide materials, polyamide A material and polyamide B material, during the process of mixing several materials, the two polyamide materials with different melting points can be melted, and the melting point temperature of the polyamide material with a higher melting point is taken to melt and mix the various materials, so that the polyamide composite material can maintain its internal fluidity during the melting process, and the polyamide B material can always remain in a liquid state by relying on the melting temperature of the polyamide A material, thereby increasing the fluidity of the polyamide composite material during preparation.
[0025] As a preferred technical solution of the present invention, polyamide A material is polyamide 56, polyamide-46 and polyamide-66, among which the melting point of polyamide 56 is 260-290°C and the density is 1.21g / cm3; the melting point of polyamide-46 is 295°C and the density is 1.18g / cm3; and the melting point of polyamide-66 is 250-260°C and the density is 0.969g / cm3.
[0026] The above technical solution can make the melting point of polyamide A material higher than that of polyamide B material during the mixing process, so that the temperature of the polyamide composite material can be controlled according to the melting point of polyamide A material during the preparation process.
[0027] As a preferred technical solution of the present invention, polyamide B is a material such as polyamide 6, polyamide 12 and polyamide-612, wherein the melting point of polyamide 6 is 215-225°C and the density is 1.13g / cm3; the melting point of polyamide 12 is 176-180°C and the density is 1.01g / cm3; and the melting point of polyamide-612 is 218°C and the density is 1.29g / cm3.
[0028] As a preferred technical solution of the present invention, the tensile strength of the glass fiber is 6.3-6.9 g / d in standard state and 5.4-5.8 g / d in wet state; the density is 2.54; the heat resistance is relatively high; and it has electrical insulation and fire shielding properties.
[0029] As a preferred technical solution of the present invention, the heat-resistant agent is one of NPMI heat-resistant agent and silica gel heat-resistant agent.
[0030] As a preferred technical solution of the present invention, the coupling agent is a kind of substance with two functional groups of different properties. The biggest feature of its molecular structure is that it contains two groups with different chemical properties in the molecule, one of which is an inorganic-philic group that is easy to react chemically with the surface of inorganic substances; the other is an organic-philic group that can react chemically with synthetic resins or other polymers or generate hydrogen bonds and dissolve therein, and is one of the KH-570 silane coupling agent and DL602 coupling agent.
[0031] As a preferred technical solution of the present invention, the antioxidant is a weak reducing agent with high chemical and physical stability or low toxicity; and the melting point of the thermal stabilizer is generally around 205°C.
[0032] As a preferred technical solution of the present invention, a method for preparing a high-strength corrosion-resistant polyamide composite material comprises the following steps:
[0033] Step 1:
[0034] Weighing polyamide B, then pouring polyamide B into a container for melting, the melting temperature is below 240°C, then taking out another set of containers to melt polyamide A, and the melting temperature is above 240°C, and then melting the glass fiber;
[0035] Step 2: Mix the melted polyamide A, polyamide B and glass fiber into a double-screw mixer, then pour the processed modified carbon nanotubes into the double-screw mixer, mix the polyamide A, polyamide B and modified carbon nanotubes at a stirring speed of 1400-1550 r / min, and keep the container temperature at about 240-300°C;
[0036] Step 3:
[0037] When the mixing work is in the first half, heat-resistant agent, coupling agent, antioxidant, heat stabilizer, colorant and other auxiliary agents are added to mix polyamide A, polyamide B and modified nano carbon tubes to form a polyamide composite material, and the heat-resistant agent, coupling agent, antioxidant, heat stabilizer, colorant and other auxiliary agents can make the polyamide composite material have other characteristics;
[0038] Step 4:
[0039] After mixing, the polyamide composite material is cut by a granulator or other equipment for storage.
[0040] As a preferred technical solution of the present invention, before the modified carbon nanotubes are used, they can be screened by ultrasonic equipment to remove impurities inside them.
[0041] The above technical solution can be used to screen the modified carbon nanotubes by ultrasonic vibration before use, so as to effectively remove impurities inside the modified carbon nanotubes, thereby increasing the overall strength of the polyamide composite material.
[0042] Compared with the prior art, the present invention has the following beneficial effects: by using two different polyamide materials, polyamide A material and polyamide B material, in the process of mixing several materials, two polyamide materials with different melting points can be melted, and the melting point temperature of the polyamide material with a higher melting point is taken to melt and mix various materials, so that the polyamide composite material can maintain its internal fluidity during the melting process, so that the polyamide B material can always maintain a liquid state by the melting temperature of the polyamide A material, thereby increasing the fluidity of the polyamide composite material during preparation;
[0043] Furthermore, by adding additives such as heat-resistant agents, coupling agents, antioxidants and heat stabilizers to the polyamide composite material, the polyamide composite material may obtain other characteristics after preparation, thereby improving the strength and corrosion resistance of the polyamide composite material;
[0044] Furthermore, by subjecting the modified carbon nanotubes to ultrasonic vibration screening before use, impurities inside the modified carbon nanotubes can be effectively removed, thereby increasing the overall strength of the polyamide composite material. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 It is a schematic diagram of the preparation process of the high-strength corrosion-resistant polyamide composite material of the present invention. DETAILED DESCRIPTION
[0046] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0047] Embodiment 1:
[0048] See also Figure 1 The present invention provides a technical solution: a high-strength corrosion-resistant polyamide composite material, prepared from the following raw materials in parts by weight:
[0049] Polyamide A: 70 parts;
[0050] Polyamide B: 15 parts;
[0051] Glass fiber: 15 parts;
[0052] Modified carbon nanotubes: 10 parts;
[0053] Heat resistant agent: 0.1-1 part;
[0054] Coupling agent: 0.1-1 part;
[0055] Antioxidant: 0.1-1 part;
[0056] Heat stabilizer: 1 part;
[0057] Colorant: 1 part;
[0058] The melting point of polyamide A is about 20°C higher than that of polyamide B, and the melting point of glass fiber is about 680°C, and the pH of glass fiber is 9-11;
[0059] The preparation method of the modified carbon nanotubes is as follows:
[0060] Step 1: Purification
[0061] Place the carbon nanotubes in a container, then pour the decomposition solution into the container, and then use ultrasound to remove impurities such as amorphous carbon and carbon nanoparticles on the carbon nanotube wall. At the same time, the carbon nanotubes will precipitate due to gravity, while impurities such as amorphous carbon and carbon nanoparticles with lower density will float to the top of the solution due to their lower density, thus leaving the surface of the carbon nanotubes.
[0062] Step 2: Mixing
[0063] The purified carbon nanotubes are placed in another container for smelting. When smelting the carbon nanotubes, the temperature needs to reach about 600°C, so that the carbon nanotubes are smelted at high temperature and cracked into carbon atoms. Then, a modification agent is added to reassemble the carbon nanotubes into modified carbon nanotubes. Then, the modified carbon nanotubes are cooled to about 500°C and smelted again.
[0064] Step 3: Cooling
[0065] The modified carbon nanotubes are placed in a cooling box, and the cooling box needs to be maintained at about -10°C so that the modified carbon nanotubes can be cooled quickly; when the modified carbon nanotubes are cooling, an ultrasonic device can be used to vibrate the inside of the container;
[0066] Due to the different specific gravity of the materials, different effects will be produced. The specific contents are shown in Table 1:
[0067]
[0068] Table 1
[0069] As can be seen from Table 1, when the polyamide B material is close to half or more of the polyamide A material, the fluidity will be improved, but when mixed with other materials, the compatibility will be poor. When the polyamide B material is less than one-third or less of the polyamide A material, it will lose a certain amount of fluidity, but the compatibility of several materials during melting will be increased.
[0070] The polyamide A material is polyamide 56, polyamide-46 and polyamide-66, wherein the melting point of polyamide 56 is 260-290°C, the melting point of polyamide-46 is 295°C, and the melting point of polyamide-66 is 250-260°C; the polyamide B material is polyamide 6, polyamide 12 and polyamide-612, wherein the melting point of polyamide 6 is 215-225°C, the melting point of polyamide 12 is 176-180°C, and the melting point of polyamide-612 is 218°C;
[0071] The tensile strength of glass fiber is 6.3-6.9g / d in standard state and 5.4-5.8g / d in wet state; the density is 2.54; the heat resistance is high; it has electrical insulation and fire shielding properties; the heat resistant agent is one of NPMI heat resistant agent and silicone heat resistant agent;
[0072] Coupling agent is a kind of substance with two functional groups of different properties. The biggest feature of its molecular structure is that it contains two groups with different chemical properties. One is an inorganic-friendly group that is easy to react chemically with the surface of inorganic substances; the other is an organic-friendly group that can react chemically with synthetic resins or other polymers or generate hydrogen bonds and dissolve in them. It is one of the KH-570 silane coupling agent and DL602 coupling agent. Antioxidants are weak reducing agents with high chemical and physical stability or low toxicity. The melting point of thermal stabilizers is generally around 205°C.
[0073] A preparation method of a high-strength corrosion-resistant polyamide composite material comprises the following steps:
[0074] Step 1:
[0075] Weighing polyamide B, then pouring polyamide B into a container for melting, the melting temperature is below 240°C, then taking out another set of containers to melt polyamide A, and the melting temperature is above 240°C, and then melting the glass fiber;
[0076] Step 2: Mix the melted polyamide A, polyamide B and glass fiber into a double-screw mixer, then pour the processed modified carbon nanotubes into the double-screw mixer, mix the polyamide A, polyamide B and modified carbon nanotubes at a stirring speed of 1400-1550 r / min, and keep the container temperature at about 240-300°C;
[0077] Step 3:
[0078] When the mixing work is in the first half, heat-resistant agent, coupling agent, antioxidant, heat stabilizer, colorant and other auxiliary agents are added to mix polyamide A, polyamide B and modified nano carbon tubes to form a polyamide composite material, and the heat-resistant agent, coupling agent, antioxidant, heat stabilizer, colorant and other auxiliary agents can make the polyamide composite material have other characteristics;
[0079] Step 4:
[0080] After mixing, the polyamide composite material is cut by a granulator or other equipment for preservation;
[0081] Before the modified carbon nanotubes are used, they can be screened by ultrasonic equipment to remove impurities inside them.
[0082] Embodiment 2:
[0083] The difference between this embodiment and embodiment 1 is that: a high-strength corrosion-resistant polyamide composite material is prepared from the following raw materials in parts by weight:
[0084] Polyamide A: 60 parts;
[0085] Polyamide B: 30 parts;
[0086] Glass fiber: 10 parts;
[0087] Modified carbon nanotubes: 10 parts;
[0088] Heat resistant agent: 0.1-1 part;
[0089] Coupling agent: 0.1-1 part;
[0090] Antioxidant: 0.1-1 part;
[0091] Heat stabilizer: 1 part;
[0092] Colorant: 1 part;
[0093] The melting point of polyamide A is about 20°C higher than that of polyamide B, and the melting point of glass fiber is about 680°C, and the pH of glass fiber is 9-11;
[0094] As can be seen from Table 1, when the polyamide B material is close to half or more of the polyamide A material, the fluidity will be improved, but when mixed with other materials, the compatibility will be poor. When the polyamide B material is less than one-third or less of the polyamide A material, it will lose a certain amount of fluidity, but the compatibility of several materials during melting will be increased.
[0095] The preparation method of the modified carbon nanotubes is as follows:
[0096] Step 1: Purification
[0097] Place the carbon nanotubes in a container, then pour the decomposition solution into the container, and then use ultrasound to remove impurities such as amorphous carbon and carbon nanoparticles on the carbon nanotube wall. At the same time, the carbon nanotubes will precipitate due to gravity, while impurities such as amorphous carbon and carbon nanoparticles with lower density will float to the top of the solution due to their lower density, thus leaving the surface of the carbon nanotubes.
[0098] Step 2: Mixing
[0099] The purified carbon nanotubes are placed in another container for smelting. When smelting the carbon nanotubes, the temperature needs to reach about 600°C, so that the carbon nanotubes are smelted at high temperature and cracked into carbon atoms. Then, a modification agent is added to reassemble the carbon nanotubes into modified carbon nanotubes. Then, the modified carbon nanotubes are cooled to about 500°C and smelted again.
[0100] Step 3: Cooling
[0101] The modified carbon nanotubes are placed in a cooling box, and the cooling box needs to be maintained at about -10°C so that the modified carbon nanotubes can be cooled quickly; when the modified carbon nanotubes are cooling, ultrasonic equipment can be used to vibrate the inside of the container.
[0102] The polyamide A material is polyamide 56, polyamide-46 and polyamide-66, wherein the melting point of polyamide 56 is 260-290°C, the melting point of polyamide-46 is 295°C, and the melting point of polyamide-66 is 250-260°C; the polyamide B material is polyamide 6, polyamide 12 and polyamide-612, wherein the melting point of polyamide 6 is 215-225°C, the melting point of polyamide 12 is 176-180°C, and the melting point of polyamide-612 is 218°C;
[0103] The tensile strength of glass fiber is 6.3-6.9g / d in standard state and 5.4-5.8g / d in wet state; the density is 2.54; the heat resistance is high; it has electrical insulation and fire shielding properties; the heat resistant agent is one of NPMI heat resistant agent and silicone heat resistant agent;
[0104] Coupling agent is a kind of substance with two functional groups of different properties. The biggest feature of its molecular structure is that it contains two groups with different chemical properties. One is an inorganic-friendly group that is easy to react chemically with the surface of inorganic substances; the other is an organic-friendly group that can react chemically with synthetic resins or other polymers or generate hydrogen bonds and dissolve in them. It is one of the KH-570 silane coupling agent and DL602 coupling agent. Antioxidants are weak reducing agents with high chemical and physical stability or low toxicity. The melting point of thermal stabilizers is generally around 205°C.
[0105] A preparation method of a high-strength corrosion-resistant polyamide composite material comprises the following steps:
[0106] Step 1:
[0107] Weighing polyamide B, then pouring polyamide B into a container for melting, the melting temperature is below 240°C, then taking out another set of containers to melt polyamide A, and the melting temperature is above 240°C, and then melting the glass fiber;
[0108] Step 2: Mix the melted polyamide A, polyamide B and glass fiber into a double-screw mixer, then pour the processed modified carbon nanotubes into the double-screw mixer, mix the polyamide A, polyamide B and modified carbon nanotubes at a stirring speed of 1400-1550 r / min, and keep the container temperature at about 240-300°C;
[0109] Step 3:
[0110] When the mixing work is in the first half, heat-resistant agent, coupling agent, antioxidant, heat stabilizer, colorant and other auxiliary agents are added to mix polyamide A, polyamide B and modified nano carbon tubes to form a polyamide composite material, and the heat-resistant agent, coupling agent, antioxidant, heat stabilizer, colorant and other auxiliary agents can make the polyamide composite material have other characteristics;
[0111] Step 4:
[0112] After mixing, the polyamide composite material is cut by a granulator or other equipment for preservation;
[0113] Before the modified carbon nanotubes are used, they can be screened by ultrasonic equipment to remove impurities inside them.
[0114] Thereby completing a series of tasks, the contents not described in detail in this specification belong to the prior art known to professional and technical personnel in this field.
[0115] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A high-strength, corrosion-resistant polyamide composite material, characterized in that: It is prepared from the following raw materials in parts by weight: Polyamide A: 20-70 parts; Polyamide B: 2-30 parts; Glass fiber: 10-30 parts; Modified carbon nanotubes: 5-15 parts; Heat resistant agent: 0.1-1 part; Coupling agent: 0.1-1 part; Antioxidant: 0.1-1 part; Heat stabilizer: 0.5-2 parts; Colorant: 0.5-2 parts; The melting point of polyamide A is about 20°C higher than that of polyamide B, and the melting point of glass fiber is about 680°C, and the pH of glass fiber is 9-11; The preparation method of the modified carbon nanotubes is as follows: Step 1: Purification Place the carbon nanotubes in a container, then pour the decomposition solution into the container, and then use ultrasound to remove impurities such as amorphous carbon and carbon nanoparticles on the carbon nanotube wall. At the same time, the carbon nanotubes will precipitate due to gravity, while impurities such as amorphous carbon and carbon nanoparticles with lower density will float to the top of the solution due to their lower density, thus leaving the surface of the carbon nanotubes. Step 2: Mixing The purified carbon nanotubes are placed in another container for smelting. When smelting the carbon nanotubes, the temperature needs to reach about 600°C, so that the carbon nanotubes are smelted at high temperature and cracked into carbon atoms. Then, a modification agent is added to reassemble the carbon nanotubes into modified carbon nanotubes. Then the modified carbon nanotubes are cooled to about 500°C and smelted further; Step 3: Cooling The modified carbon nanotubes are placed in a cooling box, and the cooling box needs to be maintained at about -10°C so that the modified carbon nanotubes can be cooled quickly; when the modified carbon nanotubes are cooling, ultrasonic equipment can be used to vibrate the inside of the container.
2. The high-strength, corrosion-resistant polyamide composite material according to claim 1, characterized in that: The polyamide A material is polyamide 56, polyamide-46, polyamide-66 and the like, wherein the melting point of polyamide 56 is 260-290°C, the melting point of polyamide-46 is 295°C, and the melting point of polyamide-66 is 250-260°C.
3. The high-strength, corrosion-resistant polyamide composite material according to claim 1, characterized in that: Polyamide B is a material such as polyamide 6, polyamide 12 and polyamide-612, wherein the melting point of polyamide 6 is 215-225°C, the melting point of polyamide 12 is 176-180°C, and the melting point of polyamide-612 is 218°C.
4. The high-strength, corrosion-resistant polyamide composite material according to claim 1, characterized in that: The tensile strength of glass fiber is 6.3-6.9 g / d in standard state and 5.4-5.8 g / d in wet state; the density is 2.54; the heat resistance is relatively high; it has electrical insulation and fire shielding properties.
5. The high-strength, corrosion-resistant polyamide composite material according to claim 1, characterized in that: The heat-resistant agent is one of NPMI heat-resistant agent and silicone heat-resistant agent.
6. The high-strength, corrosion-resistant polyamide composite material according to claim 1, characterized in that: Coupling agent is a kind of substance with two functional groups of different properties. The biggest feature of its molecular structure is that it contains two groups with different chemical properties. One is an inorganic-philic group that easily reacts chemically with the surface of inorganic substances; the other is an organic-philic group that can react chemically with synthetic resins or other polymers or generate hydrogen bonds and dissolve in them. It is one of the KH-570 silane coupling agent and DL602 coupling agent.
7. The high-strength, corrosion-resistant polyamide composite material according to claim 1, characterized in that: Antioxidants are weak reducing agents with high chemical and physical stability or low toxicity; and the melting point of heat stabilizers is generally around 205°C.
8. A method for preparing a high-strength, corrosion-resistant polyamide composite material, characterized in that: The steps include: Step 1: Weighing polyamide B, then pouring polyamide B into a container for melting, the melting temperature is below 240°C, then taking out another set of containers to melt polyamide A, and the melting temperature is above 240°C, and then melting the glass fiber; Step 2: Mix the melted polyamide A, polyamide B and glass fiber into a double-screw mixer, then pour the processed modified carbon nanotubes into the double-screw mixer, mix the polyamide A, polyamide B and modified carbon nanotubes at a stirring speed of 1400-1550 r / min, and keep the container temperature at about 240-300°C; Step 3: When the mixing work is in the first half, heat-resistant agent, coupling agent, antioxidant, heat stabilizer, colorant and other auxiliary agents are added to mix polyamide A, polyamide B and modified nano carbon tubes to form a polyamide composite material, and the heat-resistant agent, coupling agent, antioxidant, heat stabilizer, colorant and other auxiliary agents can make the polyamide composite material have other characteristics; Step 4: After mixing, the polyamide composite material is cut by a granulator or other equipment for storage.
9. The method for preparing the high-strength corrosion-resistant polyamide composite material according to claim 1, characterized in that: Before the modified carbon nanotubes are used, they can be screened by ultrasonic equipment to remove impurities inside them.
Citation Information
Patent Citations
Polyamide composite material and preparation method thereof
CN101875780B