Preparation method of graphene-based heat dissipation nano ceramic coating

Through the co-hydrolysis reaction of silicone with graphene and silicon sol, graphene-based heat dissipation nanoceramic coatings are prepared, which solves the problems of poor dispersion stability and high temperature resistance of graphene heat dissipation coatings, and improves the infrared radiation heat dissipation ability and cold and heat resistance of the coating. Impact performance, suitable for high temperature environments.

CN118931236AInactive Publication Date: 2024-11-12CHANGZHOU CARBONBO NEW MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411221556.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing graphene heat dissipation coatings have poor dispersion stability, are not resistant to high temperatures, and have poor thermal shock resistance of the coating and infrared radiation heat dissipation capabilities, which limits their application in high temperature environments.

Method used

Silicone and graphene were pre-mixed and graphene was prepared by co-hydrolysis reaction of silicone, graphene and silicon sol, and graphene was used to prepare graphene-based heat dissipation nanoceramic coatings, adjust the pH value and add stabilizers to improve dispersion and durability.

Benefits of technology

It significantly improves the dispersion of graphene in the coating and its resistance to cold and heat impact, enhances the infrared radiation heat dissipation ability and thermal conductivity of the coating, and extends the service life of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931236A_ABST
    Figure CN118931236A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of heat dissipation coating preparation, and discloses a graphene-based heat dissipation nano ceramic coating preparation method, which comprises: preparing a dispersion slurry, adjusting the pH value of the dispersion slurry, preparing an inorganic nano ceramic prepolymer, and preparing a graphene-based heat dissipation nano ceramic coating, the silane and the graphene are combined, the dispersion stability of the graphene in a system becomes good, the silane, the graphene and the silica sol are subjected to a co-hydrolysis reaction to directly generate the coating, and compared with a mode that graphene is added later to enter resin, the coating graphene is distributed more uniformly, and a co-hydrolysis product of the silane and the silica sol is uniform in dispersion and good in dispersion stability. After being baked, the coating is an inorganic nano ceramic coating which is generally brittle and easy to crack at high temperature, and through co-hydrolysis of the graphene and the inorganic nano ceramic coating, the flaky structure of the graphene improves the brittleness of the original hydrolysate, so that the cold and hot impact resistance of the coating is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of heat dissipation coating preparation, and specifically relates to a method for preparing a graphene-based heat dissipation nano-ceramic coating. Background Art

[0002] Graphene is a single-layer sheet structure composed of carbon atoms. It has the characteristics of high strength, large specific surface area, strong conductivity, etc. It also has extremely high thermal conductivity and thermal radiation coefficient. The thermal conductivity of single-layer graphene can reach 5300W / mK, which is not only better than carbon nanotubes, but also far higher than the metals with the highest thermal conductivity such as silver, copper, gold, and aluminum. Graphene also has a higher thermal radiation coefficient than metals such as copper and aluminum. Graphene has excellent thermal conductivity and heat dissipation properties. Therefore, graphene has great application prospects as a thermal conductive material for auxiliary heat dissipation.

[0003] With the development of society, the performance requirements for radiation heat dissipation materials are becoming higher and higher. For example, the coating is required to have good storage stability, good adhesion on the surface of high-temperature heaters, be able to continuously withstand high temperatures above 400°C, be smokeless and odorless at high temperatures, have a surface radiation emissivity of ≥0.9, etc., to be suitable for use in different occasions. Therefore, graphene radiation heat dissipation coatings with good storage stability, high thermal conductivity, high temperature resistance, strong resistance to cold and heat shock, good adhesion, and strong infrared radiation heat dissipation ability have gradually attracted attention.

[0004] Graphene can be used to prepare radiant heat dissipation coatings. After the coating is covered on the surface of the heat dissipation device, it can change the emissivity of the substrate surface, enhance the radiation range, and improve the heat dissipation efficiency of the device. Existing graphene radiant heat dissipation coatings are mainly prepared by stirring and mixing graphene, polymer resins and additives, and the focus is on the dispersion of graphene. However, the graphene radiant heat dissipation coatings prepared by this mixing method have certain disadvantages. Since the binder is a polymer resin, the coating has low aging resistance, UV resistance and weather resistance. In the field of high-temperature radiant heat dissipation, the coating life is very short and can only be used in the field of medium and low temperature radiant heat dissipation. In addition, the polymer binder in the coating has poor thermal conductivity and a low thermal radiation coefficient, which seriously limits the performance of graphene itself.

[0005] CN114621640 A discloses a graphene heat dissipation coating and a preparation method thereof, wherein graphene is dissolved in anhydrous ethanol, NMP and other solvents, and then modified with a silane coupling agent, and PVDF resin and acrylic resin are added to the NMP for modification to prepare the graphene heat dissipation coating. Although the graphene prepared by this preparation process has good dispersibility, it is still a process of mixing a polymer resin and modified graphene, and the coating cannot withstand high temperatures, and the PVDF resin and acrylic resin will affect the thermal conductivity and emissivity of the coating.

[0006] CN113480875 A discloses an alumina-modified graphene, a graphene heat dissipation coating and a preparation method thereof. First, alumina-modified graphene is prepared, and then the modified graphene is added to various polymer resins and various coating additives are added to obtain a highly dispersed graphene heat dissipation coating. Although this preparation method solves the dispersion problem of graphene in the coating system, the thermal conductivity of the coating is not high due to the general thermal conductivity of the polymer resin itself, and the coating cannot be used in a high temperature environment for a long time, which also limits many application scenarios, such as high-temperature heaters, high-temperature heating plates, high-temperature ovens, etc. Summary of the invention

[0007] The purpose of the present invention is to provide a method for preparing a graphene-based heat dissipation nano-ceramic coating to solve the problems in the prior art of poor dispersion stability, high temperature resistance, poor thermal shock resistance and infrared radiation heat dissipation capacity of the graphene heat dissipation coating.

[0008] In order to achieve the above object, the present invention provides the following technical solution: a method for preparing a graphene-based heat dissipation nano-ceramic coating, comprising the following steps:

[0009] Sp1: Prepare a dispersed slurry, weigh 100 parts of siloxane, add 1-50 parts of graphene, and mix the siloxane and graphene under ultrasound and stirring to obtain a highly dispersed slurry of siloxane-modified graphene;

[0010] Sp2: Adjust the pH value of the dispersed slurry. Weigh 100 parts of the siloxane-modified graphene high-dispersion slurry and add it to the reactor for stirring. During the stirring process, slowly add 0.5-10 parts of the pH regulator to adjust the pH value of the mixed solution to 2-4.

[0011] Sp3: preparing an inorganic nano-ceramic prepolymer, weighing 100 parts of a graphene high-dispersion slurry with an adjusted pH value, and slowly adding 100-500 parts of a sol while stirring the graphene high-dispersion slurry, stirring at a low speed in a sealed environment at room temperature and pressure to perform a co-hydrolysis reaction, and after the hydrolysis reaction is completed, cooling to room temperature and continuing to stir for 5-10 hours to obtain a uniformly mixed graphene inorganic nano-ceramic prepolymer;

[0012] Sp4: Prepare graphene-based heat dissipation nano-ceramic coating, add 100-500 parts of stabilizer when stirring graphene inorganic nano-ceramic prepolymer, and obtain graphene-based heat dissipation nano-ceramic coating with good storage stability.

[0013] Preferably, the siloxane is methyldimethoxysilane, methyltrimethoxysilane, propyltrimethoxysilane, propyltriethoxysilane, methyldiethoxysilane, methyltriethoxysilane, methyltetramethoxysilane, methyltetraethoxysilane, phenyltrimethoxysilane, diphenyldimethoxysilane, methylphenyldimethoxysilane, γ-(2,3-epoxypropyloxy)propyltrimethoxysilane or acryloxysilane, and the graphene is a single-layer or multi-layer graphene powder, graphene slurry or graphene cake with a sheet diameter between 0.001-10 μm.

[0014] Preferably, the pH regulator is formic acid, acetic acid, hydrochloric acid, citric acid or oxalic acid.

[0015] Preferably, the sol is silica sol, zirconium sol or aluminum sol.

[0016] Preferably, the stabilizer is methanol, ethanol, n-butanol, isopropanol or an alcohol ether solvent.

[0017] Preferably, the temperature of the reaction kettle in the Sp3 is set to 40-60°C.

[0018] The beneficial effects of the present invention are as follows:

[0019] The present invention pre-mixes silane and graphene so that silane and graphene are combined, and the dispersion stability of graphene in the system is improved. The coating is directly generated by co-hydrolysis reaction of silane, graphene and silica sol. Compared with the method of "post-adding" graphene into the resin, the distribution of graphene in the coating of the present invention is more uniform. The co-hydrolysis product of silane and silica sol is an inorganic nano-ceramic coating after baking. Usually, this coating is brittle and easily cracked at high temperature. By co-hydrolyzing graphene with the two, the flaky structure of graphene improves the brittleness of the original hydrolysis product, so that the coating's resistance to cold and hot shocks is improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a scanning electron microscope image of the silane-modified graphene of the present invention;

[0021] Figure 2 This is a scanning electron microscope image of the graphene-based high-temperature resistant radiation heat dissipation nano-ceramic paint coating of the present invention. DETAILED DESCRIPTION

[0022] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] Embodiment 1:

[0024] like Figure 1 to Figure 2 As shown, 15 parts of methyltrimethoxysiloxane, 5 parts of methyltriethoxysilane, 2 parts of γ-(2,3-epoxypropyloxy)propyltrimethoxysilane, and 1 part of graphene powder with a sheet diameter of 1 μm were weighed, ball-milled in a ball mill for 1 hour, and then transferred to a reactor, and 0.5 parts of formic acid were slowly added while stirring, and the temperature of the reactor was adjusted to 40°C, and then 32 parts of neutral silica sol were slowly added while stirring, and the co-hydrolysis reaction was carried out for 3 hours with low-speed stirring, and finally 20 parts of anhydrous ethanol and 20.5 parts of n-butanol were added, and stirred at room temperature for 1 hour to obtain a graphene-based high-temperature radiation heat dissipation ceramic coating;

[0025] Embodiment 2:

[0026] Weigh 15 parts of methyltrimethoxysiloxane, 5 parts of methyltriethoxysilane, 2 parts of γ-(2,3-epoxypropyl)propyltrimethoxysilane, and 1 part of graphene powder with a flake diameter of 5 μm, ball-mill them in a ball mill for 1 hour, then transfer them to a reactor, slowly add 0.5 parts of formic acid while stirring, adjust the temperature of the reactor to 40°C, and then slowly add 32 parts of neutral silica sol while stirring, stir at a low speed for co-hydrolysis reaction for 3 hours, finally add 20 parts of anhydrous ethanol and 20.5 parts of n-butanol, stir at room temperature for 1 hour, and obtain a graphene-based high-temperature radiation heat dissipation ceramic coating.

[0027] Embodiment 3:

[0028] Weigh 15 parts of methyltrimethoxysiloxane, 5 parts of methyltriethoxysilane, 2 parts of γ-(2,3-epoxypropyl)propyltrimethoxysilane, and 1 part of graphene powder with a flake diameter of 15 μm, ball-mill them in a ball mill for 1 hour, then transfer them to a reactor, slowly add 0.5 parts of formic acid while stirring, adjust the temperature of the reactor to 40°C, and then slowly add 32 parts of neutral silica sol while stirring, stir at a low speed for co-hydrolysis reaction for 3 hours, finally add 20 parts of anhydrous ethanol and 20.5 parts of n-butanol, stir at room temperature for 1 hour, and obtain a graphene-based high-temperature radiation heat dissipation ceramic coating.

[0029] Embodiment 4:

[0030] Weigh 15 parts of methyltrimethoxysiloxane, 5 parts of methyltriethoxysilane, 2 parts of γ-(2,3-epoxypropyl)propyltrimethoxysilane, and 5 parts of graphene powder with a flake diameter of 1 μm, ball-mill them in a ball mill for 1 hour, then transfer them to a reactor, slowly add 0.5 parts of formic acid while stirring, adjust the temperature of the reactor to 40°C, and then slowly add 32 parts of neutral silica sol while stirring, stir at a low speed for co-hydrolysis reaction for 3 hours, finally add 20 parts of anhydrous ethanol and 20.5 parts of n-butanol, stir at room temperature for 1 hour, and obtain a graphene-based high-temperature radiation heat dissipation ceramic coating.

[0031] Embodiment 5:

[0032] Weigh 15 parts of methyltrimethoxysiloxane, 5 parts of methyltriethoxysilane, 2 parts of γ-(2,3-epoxypropyl)propyltrimethoxysilane, and 1 part of graphene powder with a flake diameter of 1 μm, ball-mill them in a ball mill for 1 hour, then transfer them to a reactor, slowly add 0.5 parts of formic acid while stirring, adjust the temperature of the reactor to 40°C, and then slowly add 22 parts of neutral silica sol while stirring, stir at a low speed for co-hydrolysis reaction for 3 hours, finally add 20 parts of anhydrous ethanol and 20.5 parts of n-butanol, stir at room temperature for 1 hour, and obtain a graphene-based high-temperature radiation heat dissipation ceramic coating.

[0033] Comparative Example 1:

[0034] As shown in Table 1: 15 parts of methyltrimethoxysiloxane, 5 parts of methyltriethoxysilane, and 2 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane were weighed and added to a reactor. 0.5 parts of formic acid were slowly added while stirring. The temperature of the reactor was adjusted to 40°C. Then, 32 parts of neutral silica sol were slowly added while stirring. The co-hydrolysis reaction was carried out under low-speed stirring for 3 hours. 20 parts of anhydrous ethanol and 20.5 parts of n-butanol were added, stirred at room temperature for 1 hour, and then transferred to a ball mill. 1 part of graphene powder with a flake diameter of 1 μm was added, and ball milling was carried out for 1 hour to obtain a graphene-based high-temperature radiation heat dissipation ceramic coating.

[0035] Comparative Example 2: Weigh 12 parts of epoxy resin and 1 part of 1μm graphene powder and put them into a ball mill, then add 0.05 parts of dispersant, 0.05 parts of leveling agent and 0.05 parts of leveling agent in sequence, adjust the speed to 300r / min, and ball mill for 1 hour; add 85.6 parts of n-butanol diluent to obtain epoxy resin-based graphene radiation heat dissipation coating.

[0036] Comparative Example 3: Weigh 12 parts of fluorocarbon resin and 1 part of 1 μm graphene powder and put them into a ball mill, then add 0.05 parts of dispersant, 0.05 parts of dispersant, and 0.05 parts of leveling agent in sequence, adjust the speed to 300 r / min, and ball mill for 1 hour; add 85.6 parts of n-butanol diluent to obtain epoxy resin-based graphene radiation heat dissipation coating.

[0037] Comparative Example 4: Weigh 15 parts of methyltrimethoxysiloxane, 5 parts of methyltriethoxysilane, and 2 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, ball-mill them in a ball mill for 1 hour, then transfer them to a reactor, slowly add 0.5 parts of formic acid while stirring, adjust the temperature of the reactor to 40°C, and then slowly add 32 parts of neutral silica sol while stirring, stir at a low speed for co-hydrolysis reaction for 3 hours, finally add 20 parts of anhydrous ethanol and 20.5 parts of n-butanol, stir at room temperature for 1 hour, and obtain a high-temperature radiant heat dissipation ceramic coating.

[0038]

[0039] Table 1

[0040] It can be seen from the above table that as the diameter of graphene sheets increases in Examples 1-3, the infrared emissivity, thermal shock resistance and thermal conductivity of the coating show an increasing trend, while the storage stability shows a decreasing trend. It can be seen from Example 1 and Comparative Example 4 that the introduction of graphene can significantly improve the thermal shock resistance of the coating; the test results of Examples 1-5 and Comparative Examples 2-3 show that the method of preparing radiant heat dissipation coating by co-hydrolysis of graphene, silane and silica sol has better storage stability due to the improved graphene dispersibility; after the coating is cured, it is a graphene-based inorganic nano-composite ceramic layer, and the thermal conductivity, infrared emissivity and thermal shock resistance are much greater than those of the graphene polymer composite coating; since the emissivity, thermal conductivity and heat resistance of the polymer resin itself are relatively low, even the radiant heat dissipation coating formed after the polymer composite graphene cannot effectively exert the properties of the graphene itself.

[0041] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0042] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a graphene-based heat dissipation nano-ceramic coating, characterized in that: The following steps are involved: Sp1: preparing a dispersed slurry, mixing siloxane and graphene under ultrasound and stirring to obtain a highly dispersed slurry of siloxane-modified graphene; Sp2: Adjust the pH value of the dispersed slurry. Add the highly dispersed slurry of graphene modified by siloxane into the reactor for stirring. Slowly add the pH regulator during the stirring process to adjust the pH value of the mixed solution to 2-4. Sp3: preparing an inorganic nano-ceramic prepolymer, slowly adding the sol into the graphene high-dispersion slurry while stirring, stirring at a low speed in a sealed environment at room temperature and pressure to perform a co-hydrolysis reaction, and after the hydrolysis reaction is completed, cooling to room temperature and continuing to stir for 5-10 hours to obtain a uniformly mixed graphene inorganic nano-ceramic prepolymer; Sp4: Prepare graphene-based heat dissipation nano-ceramic coatings, add stabilizers when stirring graphene inorganic nano-ceramic prepolymers, and obtain graphene-based heat dissipation nano-ceramic coatings with good storage stability.

2. The method for preparing a graphene-based heat dissipation coating according to claim 1, characterized in that: The siloxane is set to methyldimethoxysilane, methyltrimethoxysilane, propyltrimethoxysilane, propyltriethoxysilane, methyldiethoxysilane, methyltriethoxysilane, methyltetramethoxysilane, methyltetraethoxysilane, phenyltrimethoxysilane, diphenyldimethoxysilane, methylphenyldimethoxysilane, γ-(2,3-epoxypropyloxy)propyltrimethoxysilane or acryloxysilane, and the graphene is set to a single layer, multilayer graphene powder, graphene slurry or graphene cake with a sheet diameter between 0.001-10μm.

3. The method for preparing a graphene-based heat dissipation coating according to claim 1, characterized in that: The pH regulator is formic acid, acetic acid, hydrochloric acid, citric acid or oxalic acid.

4. The method for preparing a graphene-based heat dissipation coating according to claim 1, characterized in that: The sol is set to be silica sol, zirconium sol or aluminum sol.

5. The method for preparing a graphene-based heat dissipation coating according to claim 1, characterized in that: The stabilizer is methanol, ethanol, n-butanol, isopropanol or an alcohol ether solvent.

6. The method for preparing a graphene-based heat dissipation coating according to claim 1, characterized in that: The temperature of the reactor in the Sp3 is set to 40-60°C.