Antifouling paint for display, preparation method of antifouling paint and display

By combining fluorosilicone resin with reactive diluent, coupling agent and initiator, the problem of the display coating in the prior art having high light transmittance, hardness and water contact angle is solved, and high light transmittance is achieved. Hardness and stain-resistant coating improves display effect and adhesion.

CN118931239AActive Publication Date: 2024-11-12UNIV OF ELECTRONICS SCI & TECH OF CHINA +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410989509.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

The existing display coatings are difficult to have high light transmittance, hardness and water contact angle, resulting in darker screen display effects, easy scratches, and poor anti-fingerprint effects.

Method used

Using the combination of fluorosilicone resin, reactive diluent, coupling agent and initiator, a high light transmittance, hardness and stain-resistant coating is formed through the introduction of fluorosilicone resin of a specific structure and silicon group, and the coating thickness is 0.5-0.8μm, light transmittance is greater than 95%, hardness is greater than 6H, and water contact angle is greater than 140°.

Benefits of technology

It realizes a high light transmittance, hardness and stain-resistant coating, which improves the display effect and service life of the display, has strong adhesion and simple operation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931239A_ABST
    Figure CN118931239A_ABST
Patent Text Reader

Abstract

The invention discloses an antifouling coating for a display, a preparation method of the antifouling coating and the display, and relates to the technical field of display coatings. The antifouling paint for the display comprises the following raw materials in percentage by mass: 88-95% of fluorosilicone resin, 1-8% of a reactive diluent, 3-5% of a coupling agent and 1-3% of an initiator, wherein the structural formula of the fluorosilicone resin is # imgabs 0 #, RF1 in the formula is C2-C10 perfluorinated saturated alkyl or polyfluorinated saturated alkyl, R1 is selected from polydimethylsiloxane, polydiethylsiloxane or polydi-n-butyl siloxane, and R2 and R3 are respectively and independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl or tertiary butyl. The antifouling paint has extremely strong adhesive force to a display screen, can quickly form a film on the surface of the display screen, has the coating thickness of 0.5-0.8 mu m, and has the light transmittance of more than 95%. The hardness of a film formed by the coating reaches 6H, and the coating has an extremely high water contact angle (greater than 140 degrees).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of display coatings, and in particular to an antifouling coating for a display, a preparation method thereof, and a display. Background Art

[0002] In order to overcome the defects of CRT itself (such as reflection problems and static electricity problems), large-screen monitors are mostly coated with different types of coatings on the surface of the CRT glass shell to increase anti-static, anti-radiation and anti-reflection effects. Monitors using special coatings can also enjoy high-quality images with no image distortion and balanced and bright colors. The four commonly used ones are DE coating, AGAS coating, ARAS coating, and UC coating.

[0003] The DE (Direct Etching) coating directly engraves the screen surface into an uneven shape, thereby weakening light reflection and achieving the purpose of reducing light interference.

[0004] AGAS (Anti-GlareAnti-Static: anti-glare, anti-static) coating is a silicone coating that evenly covers the surface of the screen to diffuse the reflected light, and the conductive particles contained in this coating can play an anti-static role.

[0005] ARAS (Anti-Reflection Anti-Static: anti-reflection, anti-static) coating is a multi-layer coating that can effectively prevent light reflection, making the picture clearer and brighter.

[0006] UC (UltraClear) coating is a multi-layer composite coating that can effectively prevent image distortion and improve the color balance of the image, while also having a good inhibitory effect on various interferences. When using this monitor, users can avoid dizziness and vision damage caused by the unique brightness of the cathode ray tube to the greatest extent.

[0007] However, current coatings rarely have all the characteristics of light transmittance, hardness and water contact angle, which results in the coating having a dark screen display, being easily scratched and having poor anti-fingerprint effect.

[0008] In view of this, the present invention is proposed. Summary of the invention

[0009] The object of the present invention is to provide an antifouling coating for a display, a preparation method thereof and a display.

[0010] The present invention is achieved in that:

[0011] In a first aspect, the present invention provides an antifouling coating for a display, wherein the raw materials thereof include, by mass percentage, 88%-95% of a fluorosilicone resin, 1%-8% of a reactive diluent, 3%-5% of a coupling agent, and 1%-3% of an initiator;

[0012] Wherein, the structural formula of the fluorosilicone resin is: Where R F 1 It is a perfluoro saturated alkyl group or a polyfluoro saturated alkyl group of C2 to C10, R1 is selected from a polydimethylsiloxane group, a polydiethylsiloxane group or a polydi-n-butylsiloxane group, R2 is selected from a methyl group, an ethyl group, a n-propyl group, an isopropyl group, a n-butyl group, an isobutyl group, a sec-butyl group or a tert-butyl group, and R3 is selected from a methyl group, an ethyl group, a n-propyl group, an isopropyl group, a n-butyl group, an isobutyl group, a sec-butyl group or a tert-butyl group.

[0013] In an optional embodiment, the fluorosilicone resin is selected from at least one of the following structural formulas:

[0014]

[0015] In an optional embodiment, the reactive diluent is one or more of acryloxy fluoroalkane and methacryloyloxy fluoroalkane, wherein the structural formula of the acryloxy fluoroalkane is: The structural formula of the methacryloyloxy fluoroalkane is: Where R F 2 It is a perfluoro saturated alkyl group or a polyfluoro saturated alkyl group of C4 to C8 and contains at least one branched trifluoromethyl group.

[0016] In an optional embodiment, the reactive diluent is selected from at least one of dodecafluoroheptyl acrylate, dodecafluoroheptyl methacrylate, octafluoropentyl acrylate, perfluorobutyl acrylate and tridecafluorooctyl methacrylate.

[0017] In an optional embodiment, the initiator includes at least one of tert-butyl perbenzoate, acetophenone peroxide and di-tert-butyl peroxide.

[0018] In an optional embodiment, the coupling agent includes at least one of a silicon coupling agent and a titanate coupling agent.

[0019] In a second aspect, the present invention provides a method for preparing an antifouling coating for a display, comprising: mixing the raw materials of the antifouling coating for a display as described in any one of the aforementioned embodiments.

[0020] In an optional embodiment, the preparation method of the fluorosilicone resin comprises: mixing hydrogen-containing silicone oil and fluoroalkyl vinyl ether, heating to 80-120° C., adding chloroplatinic acid as a catalyst, and keeping the temperature for 2-4 hours to obtain the obtained product, wherein the structural formula of the hydrogen-containing silicone oil is: The structural formula of the fluoroalkyl vinyl ether is: Where R F 1 is a C2-C10 perfluoro saturated alkyl or polyfluoro saturated alkyl group, R1 is selected from a polydimethylsiloxane group, a polydiethylsiloxane group or a polydi-n-butylsiloxane group, R2 is selected from a methyl group, an ethyl group, a n-propyl group, an isopropyl group, a n-butyl group, an isobutyl group, a sec-butyl group or a tert-butyl group, and R3 is selected from a methyl group, an ethyl group, a n-propyl group, an isopropyl group, a n-butyl group, an isobutyl group, a sec-butyl group or a tert-butyl group;

[0021] Preferably, the hydrogen-containing silicone oil is selected from at least one of the following structural formulas:

[0022]

[0023] Preferably, the fluoroalkyl vinyl ether is selected from at least one of the following structural formulas:

[0024]

[0025] In an optional embodiment, the mass ratio of the hydrogen-containing silicone oil to the fluoroalkyl vinyl ether is 1:2-8;

[0026] And / or, the hydrogen content of the hydrogen-containing silicone oil is 0.5-1.8%;

[0027] And / or, the amount of the catalyst chloroplatinic acid used is 5 to 100 ppm.

[0028] In a third aspect, the present invention provides a display, which is coated with the antifouling coating for a display as described in any one of the aforementioned embodiments, wherein the coating thickness of the antifouling coating for a display is 0.5-0.8 μm;

[0029] and / or, the light transmittance of the coating is greater than 95%;

[0030] And / or, the hardness of the coating after film formation is greater than 6H;

[0031] And / or, the water contact angle of the coating is 140° to 162°.

[0032] The present invention has the following beneficial effects:

[0033] The antifouling coating for display provided by the present invention is prepared by combining a fluorosilicone resin of a specific structure with an active diluent, a coupling agent and an initiator, wherein the fluorosilicone resin contains a fluorocarbon chain and a silicon group at the same time. Due to the introduction of a long-chain and branched fluorine-containing group, the fluorine-containing group is enriched on the surface of the fluorosilicone resin after film formation to form a good hydrophobic and oleophobic interface. In addition, due to the introduction of the siloxane group, the crystallinity of the polymer is reduced, and the light transmittance is higher after film formation. At the same time, the adhesion between the coating and the substrate is increased, and the impact strength of the film is also improved. The preparation method of the antifouling coating for display provided by the present invention is simple and easy to operate. The prepared antifouling coating for display has extremely strong adhesion to the display screen (glass, polycarbonate, PET, etc.), can form a film quickly on the surface of the display, and the coating has a thickness of 0.5-0.8 μm and a light transmittance of more than 95%. The coating reaches a hardness of 6H after film formation and has an extremely high water contact angle (>140°). DETAILED DESCRIPTION

[0034] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0035] The invention provides an antifouling coating for a display. The raw materials thereof include 88%-95% of fluorosilicone resin, 1%-8% of active diluent, 3%-5% of coupling agent and 1%-3% of initiator in terms of mass percentage.

[0036] In the present invention, the fluorosilicone resin and the reactive diluent are selected so as to achieve a better coordination effect of the two.

[0037] Among them, the structural formula of fluorosilicone resin is: Where R F 1 It is a perfluoro saturated alkyl group or a polyfluoro saturated alkyl group of C2 to C10, R1 is selected from a polydimethylsiloxane group, a polydiethylsiloxane group or a polydi-n-butylsiloxane group, R2 is selected from a methyl group, an ethyl group, a n-propyl group, an isopropyl group, a n-butyl group, an isobutyl group, a sec-butyl group or a tert-butyl group, and R3 is selected from a methyl group, an ethyl group, a n-propyl group, an isopropyl group, a n-butyl group, an isobutyl group, a sec-butyl group or a tert-butyl group.

[0038] Specifically, the fluorosilicone resin is selected from at least one of the following structural formulas:

[0039]

[0040] The active diluent is one or more of acryloyloxy fluoroalkane and methacryloyloxy fluoroalkane, wherein the structural formula of acryloyloxy fluoroalkane is: The structural formula of methacryloyloxy fluoroalkane is: Where R F 2 The active diluent is selected from at least one of dodecafluoroheptyl acrylate, dodecafluoroheptyl methacrylate, octafluoropentyl acrylate, perfluorobutyl acrylate and tridecafluorooctyl methacrylate.

[0041] From the selection of fluorosilicone resin and reactive diluent in the present invention, it can be seen that the fluorosilicone resin contains fluorocarbon chains and silicon groups, and the reactive diluent also contains fluorocarbon chains. The system can be cured and cross-linked during thermal curing without losing the performance of the fluorosilicone resin.

[0042] Further, the initiator in the present invention includes but is not limited to at least one of tert-butyl perbenzoate, acetophenone peroxide and di-tert-butyl peroxide. The coupling agent includes but is not limited to at least one of a silicon coupling agent and a titanate coupling agent, wherein the silicon coupling agent may be, for example, silicon coupling agent 550 and silicon coupling agent 560. The titanate coupling agent may be, for example, tetrabutyl titanate.

[0043] In addition, the present invention provides a method for preparing an antifouling coating for a display, comprising: mixing the raw materials of the antifouling coating for a display.

[0044] Specifically, the steps include:

[0045] S1. Prepare fluorosilicone resin.

[0046] The hydrogen-containing silicone oil and fluoroalkyl vinyl ether are mixed in a mass ratio of 1:2-8, the hydrogen content of the hydrogen-containing silicone oil is 0.5-1.8%, the temperature is raised to 80-120°C, chloroplatinic acid catalyst is added, the amount of chloroplatinic acid catalyst is 5-100ppm, and the reaction is kept warm for 2-4h to obtain the product.

[0047] Among them, the structural formula of hydrogen silicone oil is: The structural formula of fluoroalkyl vinyl ether is: Where R F 1 is a C2-C10 perfluoro saturated alkyl or polyfluoro saturated alkyl group, R1 is selected from a polydimethylsiloxane group, a polydiethylsiloxane group or a polydi-n-butylsiloxane group, R2 is selected from a methyl group, an ethyl group, a n-propyl group, an isopropyl group, a n-butyl group, an isobutyl group, a sec-butyl group or a tert-butyl group, and R3 is selected from a methyl group, an ethyl group, a n-propyl group, an isopropyl group, a n-butyl group, an isobutyl group, a sec-butyl group or a tert-butyl group;

[0048] Wherein, the hydrogen-containing silicone oil is selected from at least one of the following structural formulas:

[0049]

[0050] The fluoroalkyl vinyl ether is selected from at least one of the following structural formulas:

[0051]

[0052] S2. Mixing raw materials.

[0053] Mix 88-95 parts of fluorosilicone resin, 3-10 parts of reactive diluent, 1-3 parts of initiator and 3-5 parts of coupling agent, and stir at room temperature for 3-5 minutes.

[0054] The prepared antifouling coating has strong adhesion and can be applied to the surface of a display. The coating thickness of the antifouling coating for a display is 0.5-0.8 μm; the light transmittance of the coating is greater than 95%; the hardness of the coating after film formation is greater than 6H; and the water contact angle of the coating is 140° to 162°.

[0055] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0056] Example 1

[0057] This embodiment provides an antifouling coating for a display, wherein the raw materials thereof include 190 g of fluorosilicone resin FS, 4 g of dodecafluoroheptyl acrylate, 3 g of tetrabutyl titanate, and 3 g of acetophenone peroxide.

[0058] The preparation method comprises: adding the above raw materials according to the mass ratio and stirring and dissolving them at room temperature to obtain the product.

[0059] The preparation method of fluorosilicone resin FS1 comprises: mixing 100 g of hydrogen-containing silicone oil with a hydrogen content of 1% and fluoroalkyl vinyl ether 565g of the mixture was stirred and mixed, the temperature was raised to 100°C, 5g of chloroplatinic acid as a catalyst was added, and the mixture was kept warm for reaction for 3 hours.

[0060] Example 2

[0061] This embodiment provides an antifouling coating for a display, wherein the raw materials include 8 g of fluorosilicone resin FS28, 6 g of dodecafluoroheptyl methacrylate, 5 g of silicon coupling agent 550, and 1 g of di-tert-butyl peroxide.

[0062] The preparation method comprises: adding the above raw materials according to the mass ratio and stirring and dissolving them at room temperature to obtain the product.

[0063] The preparation method of fluorosilicone resin FS1 comprises: mixing 100 g of hydrogen-containing silicone oil with a hydrogen content of 1.6% and fluoroalkyl vinyl ether 340g of the mixture was stirred and mixed, the temperature was raised to 80°C, 0.8g of chloroplatinic acid as a catalyst was added, and the mixture was kept warm for reaction for 3 hours.

[0064] Example 3

[0065] This embodiment provides an antifouling coating for a display, wherein the raw materials include 4 g of fluorosilicone resin FS39, 1 g of octafluoropentyl acrylate, 3 g of silicon coupling agent 560, and 2 g of acetophenone peroxide.

[0066] The preparation method comprises: adding the above raw materials according to the mass ratio and stirring and dissolving them at room temperature to obtain the product.

[0067] The preparation method of fluorosilicone resin FS1 comprises: mixing 100 g of hydrogen-containing silicone oil with a hydrogen content of 1.2% and fluoroalkyl vinyl ether 200g of the mixture was stirred and mixed, the temperature was raised to 120°C, 12g of chloroplatinic acid as a catalyst was added, and the mixture was kept warm for reaction for 3 hours.

[0068] Example 4

[0069] This embodiment provides an antifouling coating for a display, wherein the raw materials include 490 g of fluorosilicone resin FS, 5 g of perfluorobutyl acrylate, 3 g of silicon coupling agent 550, and 2 g of tert-butyl peroxybenzoate.

[0070] The preparation method comprises: adding the above raw materials according to the mass ratio and stirring and dissolving them at room temperature to obtain the product.

[0071] The preparation method of fluorosilicone resin FS1 comprises: mixing 100 g of hydrogen-containing silicone oil with a hydrogen content of 1.5% and fluoroalkyl vinyl ether 710g was stirred and mixed, the temperature was raised to 100°C, 9g of chloroplatinic acid as catalyst was added, and the reaction was kept warm for 3 hours.

[0072] Example 5

[0073] This embodiment provides an antifouling coating for a display, wherein the raw materials include 3 g of fluorosilicone resin FS19, 3 g of tridecafluorooctyl methacrylate, 3 g of silicon coupling agent 550, and 1 g of di-tert-butyl peroxide.

[0074] The preparation methods of the antifouling coating for display and the fluorosilicone resin FS1 are the same as those in Example 1.

[0075] Example 6

[0076] This embodiment provides an antifouling coating for a display, wherein the raw materials include 5 g of fluorosilicone resin FS39, 1 g of tridecafluorooctyl methacrylate, 3 g of silicon coupling agent 550, and 1 g of di-tert-butyl peroxide.

[0077] The preparation methods of the antifouling coating for display and the fluorosilicone resin FS3 are the same as those in Example 3.

[0078] Comparative Example 1

[0079] This comparative example is basically the same as Example 1, except that the fluorosilicone resin in this comparative example is a free radical polymerization copolymer of methyl methacrylate, butyl acrylate, acrylic acid, vinyl triethoxysilane, and hexafluorobutyl methacrylate, and its preparation method is to dissolve a certain amount of initiator in a certain amount of mixed solvent. In a four-necked bottle equipped with a stirrer, a reflux condenser, a thermometer, and a constant pressure dropping funnel, methyl methacrylate, butyl acrylate, acrylic acid, vinyl triethoxysilane, hexafluorobutyl methacrylate and a mixed solvent are added in sequence, stirred and mixed, heated to 100°C under nitrogen protection, and the remaining initiator is slowly added dropwise to the mixed solution, kept warm for a certain period of time, and discharged.

[0080] Comparative Example 2

[0081] This comparative example is substantially the same as Example 1, except that the mass ratio of the hydrogen-containing silicone oil to the fluoroalkyl vinyl ether in this comparative example is 1:1, that is, the mass of the added fluoroalkyl vinyl ether is 100 g.

[0082] Comparative Example 3

[0083] This comparative example is substantially the same as Example 1, except that the mass ratio of hydrogen-containing silicone oil to fluoroalkyl vinyl ether in this comparative example is 1:10, that is, the mass of the added fluoroalkyl vinyl ether is 1000 g.

[0084] Comparative Example 4

[0085] This comparative example is substantially the same as Example 1, except that the active diluent in this comparative example is butyl acrylate.

[0086] Comparative Example 5

[0087] This comparative example is basically the same as Example 1, except that the amount of raw materials used in this comparative example is different. The raw materials in this comparative example include 80 g of fluorosilicone resin FS1, 10 g of dodecafluoroheptyl acrylate, 6 g of tetrabutyl titanate and 4 g of acetophenone peroxide.

[0088] Comparative Example 6

[0089] This comparative example is basically the same as Example 1, except that the amount of raw materials used in this comparative example is different. The raw materials in this comparative example include 97 g of fluorosilicone resin FS1, 0.5 g of dodecafluoroheptyl acrylate, 2 g of tetrabutyl titanate and 0.5 g of acetophenone peroxide.

[0090] Experimental example

[0091] The antifouling coatings for displays prepared in the above Examples 1-6 and Comparative Examples 1-6 were applied to the surface of the display, and the transmittance, hardness and water contact angle were tested after coating. The transmittance test method includes GB / T 2410-2008 Transparent Plastic Transmittance and Haze Test; the hardness test method includes GB / T 6739-2022 Paint and Varnish Pencil Method for Determining Paint Film Hardness; the water contact angle test method includes GB / T 30447-2013 Nanofilm Contact Angle Measurement Method or GB / T30693-2014 Plastic Film and Water Contact Angle Measurement. The test results are as follows:

[0092] Example Coating thickness / μm Light transmittance / % Film hardness Water contact angle / ° Example 1 0.5 97 >6H 160 Example 2 0.58 97 >6H 145 Example 3 0.77 96 >6H 146 Example 4 0.6 97 >6H 155 Example 5 0.8 95 >6H 162 Example 6 0.8 95 >6H 140 Comparative Example 1 0.5 87 5H 106 Comparative Example 2 0.5 91 5H 105 Comparative Example 3 0.5 94 2H 128 Comparative Example 4 0.5 96 5H 124 Comparative Example 5 0.5 82 4H 110 Comparative Example 6 0.5 85 2H 133

[0093] As can be seen from the table above, the fluorosilicone resin after thermal curing and cross-linking has a very high water contact angle and paint film hardness. And because the silicon-containing group is used as the main chain structure, the light transmittance and hardness of the paint film are greatly improved, and it helps to improve adhesion.

[0094] Specifically, Examples 1-6 of the present invention all have extremely high light transmittance, paint film hardness and water contact angle. In Comparative Example 1, a conventional method is used to prepare fluorosilicone resin, and its light transmittance, paint film hardness and water contact angle are significantly lower than those in Example 1. The reason is that the main chain is a hydrocarbon chain and all functional groups are in the side chain. The mass ratio of hydrogen-containing silicone oil to fluoroalkyl vinyl ether in Comparative Examples 2 and 3 is not within the range of 1:2-8 in the present application. When the amount of fluoroalkyl vinyl ether is too low, the light transmittance, paint film hardness and water contact angle will be significantly reduced. When the amount of fluoroalkyl vinyl ether is too high, not only will the performance not be improved, but the light transmittance, paint film hardness and water contact angle will be reduced, especially the paint film hardness can only reach 2H. The use of other active diluents that do not contain fluorocarbon chains in Comparative Example 4 will result in poor curing and cross-linking effects of the system and affect the performance of the fluorosilicone resin, thereby reducing the light transmittance, paint film hardness and water contact angle. In Comparative Examples 5 and 6, the dosage of the raw materials was adjusted, especially too little or too much fluorosilicone resin, which would result in significantly worse effects than Example 1.

[0095] In summary, the antifouling coating for displays provided by the present invention is prepared by combining a fluorosilicone resin of a specific structure with an active diluent, a coupling agent and an initiator, wherein the fluorosilicone resin contains both a fluorocarbon chain and a silicon base. The fluorosilicone resin of this structure forms a dense film after heat curing and cross-linking, and the fluorine-containing segments aggregate on the surface during film formation to provide antifouling ability. The introduction of silicon improves adhesion while reducing crystallinity and improving transmittance. The preparation method of the antifouling coating for displays provided by the present invention is simple and easy to operate. The prepared antifouling coating for displays has extremely strong adhesion to display screens (glass, polycarbonate, PET, etc.), can quickly form a film on the surface of the display, with a coating of 0.5-0.8μm and a light transmittance of more than 95%. The coating reaches a hardness of 6H after film formation and has an extremely high water contact angle (>140°).

[0096] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. An antifouling coating for a display, It is characterized in that The raw materials include 88%-95% of fluorosilicone resin, 1%-8% of active diluent, 3%-5% of coupling agent and 1%-3% of initiator by mass percentage; Wherein, the structural formula of the fluorosilicone resin is: Where R F 1 It is a perfluoro saturated alkyl group or a polyfluoro saturated alkyl group of C2 to C10, R1 is selected from a polydimethylsiloxane group, a polydiethylsiloxane group or a polydi-n-butylsiloxane group, R2 is selected from a methyl group, an ethyl group, a n-propyl group, an isopropyl group, a n-butyl group, an isobutyl group, a sec-butyl group or a tert-butyl group, and R3 is selected from a methyl group, an ethyl group, a n-propyl group, an isopropyl group, a n-butyl group, an isobutyl group, a sec-butyl group or a tert-butyl group.

2. The antifouling coating for display according to claim 1, It is characterized in that The fluorosilicone resin is selected from at least one of the following structural formulas:

3. The antifouling coating for display according to claim 2, It is characterized in that The active diluent is one or more of acryloxy fluoroalkane and methacryloyloxy fluoroalkane, wherein the structural formula of the acryloxy fluoroalkane is: The structural formula of the methacryloyloxy fluoroalkane is: Where R F 2 It is a perfluoro saturated alkyl group or a polyfluoro saturated alkyl group of C4 to C8 and contains at least one branched trifluoromethyl group.

4. The antifouling coating for display according to claim 3, It is characterized in that The active diluent is selected from at least one of dodecafluoroheptyl acrylate, dodecafluoroheptyl methacrylate, octafluoropentyl acrylate, perfluorobutyl acrylate and tridecafluorooctyl methacrylate.

5. The antifouling coating for display according to claim 1, It is characterized in that The initiator includes at least one of tert-butyl perbenzoate, acetophenone peroxide and di-tert-butyl peroxide.

6. The antifouling coating for display according to claim 1, It is characterized in that The coupling agent includes at least one of a silicon coupling agent and a titanate coupling agent.

7. A method for preparing an antifouling coating for a display, It is characterized in that It includes: The raw materials of the antifouling coating for display according to any one of claims 1 to 6 are mixed.

8. The method for preparing the antifouling coating for display according to claim 7, It is characterized in that The preparation method of the fluorosilicone resin comprises: mixing hydrogen-containing silicone oil and fluoroalkyl vinyl ether, heating to 80-120° C., adding chloroplatinic acid as a catalyst, and keeping the temperature for 2-4 hours to obtain the obtained product, wherein the structural formula of the hydrogen-containing silicone oil is: The structural formula of the fluoroalkyl vinyl ether is: Where R F 1 is a C2-C10 perfluoro saturated alkyl or polyfluoro saturated alkyl group, R1 is selected from a polydimethylsiloxane group, a polydiethylsiloxane group or a polydi-n-butylsiloxane group, R2 is selected from a methyl group, an ethyl group, a n-propyl group, an isopropyl group, a n-butyl group, an isobutyl group, a sec-butyl group or a tert-butyl group, and R3 is selected from a methyl group, an ethyl group, a n-propyl group, an isopropyl group, a n-butyl group, an isobutyl group, a sec-butyl group or a tert-butyl group; Preferably, the hydrogen-containing silicone oil is selected from at least one of the following structural formulas: Preferably, the fluoroalkyl vinyl ether is selected from at least one of the following structural formulas:

9. The method for preparing the antifouling coating for display according to claim 8, It is characterized in that The mass ratio of the hydrogen-containing silicone oil to the fluoroalkyl vinyl ether is 1:2-8; And / or, the hydrogen content of the hydrogen-containing silicone oil is 0.5-1.8%; And / or, the amount of the catalyst chloroplatinic acid used is 5 to 100 ppm.

10. A display, It is characterized in that It is coated with the antifouling coating for display according to any one of claims 1 to 6, wherein the coating thickness of the antifouling coating for display is 0.5 to 0.8 μm; and / or, the light transmittance of the coating is greater than 95%; And / or, the hardness of the coating after film formation is greater than 6H; And / or, the water contact angle of the coating is 140° to 162°.

Citation Information

Patent Citations

  • Fluorine silicon resin, preparation method thereof and antifouling paint

    CN101775144A

  • Low-surface energy fluorosilicone polymer and preparation method thereof

    CN102134323A

  • Crosslinkable fluorosilicone resin, painting and super-amphiphobic coating prepared by same

    CN103408762A

  • Paint composition, paint, coating, silica coating, article with coating and method for forming coating on surface of substrate

    CN109096915A

  • Substrate having complex hard coat layer where antifouling coating agent is coated on hard coat layer, and a method of forming the same

    JP2007297543A