Acrylic polyurethane finish paint and preparation method thereof
By using heat-sensitive acrylic monomers, polyurethane prepolymers and isocyanate crosslinkers in acrylic polyurethane topcoats, combined with ultraviolet and infrared curing technologies, the problem of degradation of performance and long curing time of acrylic polyurethane topcoats in extreme environments is solved. It achieves high-efficiency, low-energy coating curing and excellent mechanical properties and temperature feedback effects.
Patent Information
- Application Number
- CN202411144764.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-12
AI Technical Summary
The existing acrylic polyurethane topcoat has deteriorated performance in extreme environments and has long curing time, which affects production efficiency and energy consumption, limiting its application range.
Using heat-sensitive acrylic monomers, polyurethane prepolymers and isocyanate crosslinkers, combined with UV and infrared curing technology, optimize the ratio and curing process, form a coating with high mechanical strength and temperature resistance, and passes through chromophores Provides visual feedback on temperature variation.
It significantly shortens curing time, improves production efficiency, reduces energy consumption, enhances the mechanical strength and temperature resistance of the coating, provides instant feedback on temperature change and better surface flatness and smoothness.
Smart Images

Figure CN118931241A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coatings, in particular to an improved acrylic polyurethane topcoat and a preparation method thereof. Background Art
[0002] Among existing coating technologies, acrylic polyurethane topcoats are widely used in protective and decorative coatings due to their excellent weather resistance and mechanical strength. However, although existing products provide certain protective effects, their effectiveness and application range are limited.
[0003] First, the performance of existing acrylic polyurethane topcoats will significantly decrease under extreme environmental conditions, such as high or low temperatures, which affects their application in specific industries. Second, the curing time of the topcoat is long, which not only affects production efficiency but also increases energy consumption, especially in large-scale industrial applications.
[0004] Based on this, a kind of acrylic polyurethane topcoat and preparation method thereof are needed. Summary of the invention
[0005] To achieve the above object, the present invention provides the following solution: an acrylic polyurethane topcoat, the topcoat comprising the following components in weight proportion:
[0006] Heat sensitive acrylic monomer: 5-10%
[0007] Polyurethane prepolymer: 40-50%
[0008] Crosslinking agent: 3-5%
[0009] Chromophore: 2-4%
[0010] Organic solvents and other auxiliary additives: balance
[0011] Wherein, the heat-sensitive acrylic monomer is a chromophore with thermochromic properties, which can change its color when a specific temperature threshold is reached;
[0012] The polyurethane prepolymer is used to form the main structure of the coating and provide basic mechanical properties and durability;
[0013] The cross-linking agent is used to enhance the thermal stability and mechanical strength of the topcoat, ensuring the integrity and durability of the coating under temperature changes;
[0014] The chromophore is a thermosensitive compound that can undergo a chemical structural change at a specific temperature, thereby causing a color change, which is used to provide visual feedback to indicate temperature changes;
[0015] The solvent and other auxiliary additives are used to adjust the viscosity, fluidity and drying time of the coating to facilitate the application and film-forming process of the coating.
[0016] In some embodiments, the heat-sensitive acrylic monomer is first premixed with the modified chromophore in a high shear mixer to ensure that the chromophore is evenly dispersed in the monomer, and then the polyurethane prepolymer is gradually added to the mixture and stirred at 60° C. for 2 hours to form a uniform reaction mixture.
[0017] In some embodiments, a specific proportion of a cross-linking agent is added to the mixed heat-sensitive acrylic monomer and polyurethane prepolymer, wherein the cross-linking agent is selected from isocyanates to ensure the formation of a strong three-dimensional network structure in the subsequent curing process, thereby improving the mechanical properties and temperature resistance of the coating. The added organic solvent and other auxiliary additives include a leveling agent, and the proportion of the additive in the final mixture is 10% of the total weight, which is used to adjust the fluidity and surface tension of the final coating to obtain ideal surface smoothness and glossiness.
[0018] In some embodiments, the curing process of the coating is carried out in an environment heated to 80° C. for 4 hours, during which the temperature is gradually increased to control the curing speed and cross-linking density to ensure the uniformity of the coating and the final stable performance.
[0019] In some embodiments, before the mixture is cured, high-speed centrifugation is performed to remove unreacted monomers and formed bubbles. This step ensures the density and smoothness of the coating and reduces the need for subsequent treatment.
[0020] In some embodiments, ultraviolet curing technology is used, wherein the ultraviolet intensity is set to 500mW / cm 2 The irradiation time is 5 minutes, which quickly cures the coating and improves production efficiency while ensuring that the physical and chemical properties of the coating meet the expected standards. Infrared heating is used during the curing process to optimize the cross-linking reaction of the coating. The use of infrared light penetrates deep into the coating and heats it evenly to avoid excessive curing of the surface and insufficient reaction inside.
[0021] According to the specific embodiments provided by the present invention, the present invention discloses the following technical effects:
[0022] First, the present invention introduces a heat-sensitive acrylic monomer, so that the topcoat can undergo a significant color change when a specific temperature threshold is reached, providing instant visual feedback. This feature makes the topcoat very suitable for safety-sensitive applications, such as being able to promptly remind operators and maintenance personnel to take corresponding treatment measures in an overheated or overcooled environment;
[0023] 2. The present invention significantly shortens the curing time of the coating by using isocyanate crosslinking agents combined with ultraviolet and infrared curing technologies. Compared with traditional thermal curing systems, the dual curing strategy of the present invention reduces the time and energy consumption required in the curing process, thereby improving overall production efficiency and reducing costs.
[0024] 3. By optimizing the ratio of the polyurethane prepolymer to the isocyanate crosslinking agent and precisely controlling the temperature and time during the curing process, the topcoat of the present invention has higher mechanical strength and better temperature resistance, and can effectively resist extreme temperatures and mechanical wear.
[0025] Fourth, the present invention adds a leveling agent with an optimized ratio to the topcoat, which effectively improves the surface flatness and smoothness of the coating, enhances the aesthetics of the coating, and also improves its anti-pollution and cleaning and maintenance capabilities. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0027] Figure 1 The present invention is a flow chart for preparing an acrylic polyurethane topcoat. DETAILED DESCRIPTION
[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0030] Example
[0031] like Figure 1 As shown, an acrylic polyurethane topcoat in this embodiment includes the following components in weight proportion:
[0032] Heat sensitive acrylic monomer: 5-10%
[0033] Thermosensitive acrylic monomers are one of the key components of topcoats. The selected thermosensitive monomers contain chromophores that can undergo structural changes at specific temperatures;
[0034] The following are several heat-sensitive monomers used in this type of topcoat:
[0035] Selection of Spirochrome derivatives: organic compounds commonly used in thermochromic systems, which can change from colorless to colored and vice versa at a certain temperature through a ring-opening reaction, allowing the acrylic polyurethane topcoat to achieve temperature-sensitive color changes, suitable for applications such as safety marking and temperature warnings.
[0036] Selection of styrene-based heat-sensitive monomers: Specific styrene derivatives polymerize or depolymerize under the action of heat, thereby changing their physical properties. This allows acrylic polyurethane topcoat to have a unique ability to change hardness in a temperature-sensitive manner. It is used for surface protection in variable temperature environments, such as providing higher flexibility at low temperatures and hardening at high temperatures to protect the base layer.
[0037] Select monomers combined with thermosensitive pigments: Combine thermosensitive pigments with acrylic groups through chemical bonding to form copolymerizable monomers, so that the acrylic polyurethane topcoat can intuitively display temperature changes and directly reflect the temperature through changes in color.
[0038] Selection of methylene blue modified monomer: a reversible redox reaction will occur under the influence of heat, affecting the color display, so that the acrylic polyurethane topcoat has a unique temperature-sensitive color change characteristic, which is used in occasions that need to respond quickly to environmental changes, such as safety signs in high-temperature working areas.
[0039] When the temperature of the environment in which the topcoat is located reaches the preset threshold, the chromophore undergoes chemical changes, causing a significant change in color, thereby achieving a visual indication of the temperature, specifically:
[0040] Closed-ring state: At lower temperatures, the chromophore molecules maintain a stable closed-ring state, in which the key functional groups for color change are locked in a non-conjugated system, limiting their color expression;
[0041] Temperature trigger: When the ambient temperature reaches the preset threshold, the chemical bonds inside the molecules break due to the surge in thermal energy, resulting in a transition from a closed loop to an open loop;
[0042] Open ring state: After the ring is opened, the previously restricted functional groups participate in the conjugated system, which significantly changes the electronic structure and light absorption characteristics of the molecule, resulting in the appearance or change of color.
[0043]
[0044] Color change description: Describe the color performance of the coating at different temperatures. The color changes from colorless and transparent to dark purple, showing the color change caused by the ring opening of the chromophore due to the increase in temperature;
[0045] Hardness (ShoreD): As the temperature increases, the hardness of the topcoat decreases slightly, showing that the material softens under the action of heat;
[0046] Abrasion resistance (number of cycles): Indicates the number of cycles that the topcoat can withstand on a standard abrasion test machine. The data shows that as the temperature increases, the abrasion resistance decreases slightly, which is related to the decrease in hardness.
[0047] Transparency change (%): As the temperature increases, the transparency of the topcoat gradually decreases, indicating that the chemical changes of the chromophores at high temperatures affect the optical properties of the material;
[0048] Polyurethane prepolymer: 40-50%
[0049] Polyurethane prepolymer is the basic material that constitutes the main body of the coating. It not only provides the required mechanical strength and durability, but also ensures good adhesion and flexibility of the coating. Polyurethane makes the topcoat suitable for outdoor applications and harsh environments due to its excellent weather resistance and chemical resistance.
[0050] Polyurethane prepolymers are obtained by prepolymerizing isocyanates and polyols, which provide the core physical and chemical properties required for coatings, including:
[0051] Mechanical strength: Polyurethane prepolymers can form a high-strength polymer network to ensure that the coating has sufficient tear and wear resistance;
[0052] Durability: The cross-linked structure of the prepolymer provides the coating with excellent weather resistance, allowing the topcoat to resist environmental factors such as UV rays, rain and temperature changes;
[0053] Good adhesion and flexibility: The chemical structure of polyurethane enables it to adhere well to a variety of substrate surfaces while remaining flexible enough to prevent the coating from cracking or peeling;
[0054]
[0055] Tensile strength test: Use a standard tensile testing machine to stretch the cured polyurethane sample and measure the maximum stress at break;
[0056] Adhesion test: The cross-cut method is used to cut a grid on the coating surface and then test the peeling of the coating with an adhesive tape;
[0057] Weathering test: The samples are aged in a simulated UV and humidity cycle environment to test their color and gloss retention;
[0058] Flexibility test: The coating is applied to a metal plate and the plate is bent to test whether the coating will crack due to bending;
[0059] Polyurethane prepolymers provide topcoats with excellent mechanical properties, durability and serviceability.
[0060] Crosslinking agent: 3-5%
[0061] The addition of crosslinking agents is used to improve the thermal stability and mechanical strength of the coating. Isocyanates or multifunctional crosslinking agents are selected to react with polyurethane chains during the curing process of the coating to form a three-dimensional crosslinking network. This structure can remain stable at high temperatures and reduce the movement or deconstruction of polymer chains caused by thermal energy, thereby maintaining the structural integrity and surface smoothness of the coating. The crosslinking network increases the rigidity and tensile strength of the material, allowing the coating to withstand greater mechanical stress without cracking or deformation. It also improves impact resistance and wear resistance, helping the coating maintain its structural integrity and performance when subjected to temperature changes;
[0062] Organic solvents and other auxiliary additives: The balance is made up of appropriate amounts of organic solvents and leveling agents. Organic solvents are used to adjust the viscosity and fluidity of the coating so that it can reach a fluidity suitable for spraying, brushing or other construction methods, helping the coating to form a uniform coating on the surface of the substrate to prevent sagging or uneven coating, while the leveling agent improves the surface quality of the coating and accelerates the curing process.
[0063] in,
[0064] Thermosensitive acrylic monomers are chromophores with thermochromic properties, which can change their color when a certain temperature threshold is reached;
[0065] Polyurethane prepolymers are used to form the main structure of the coating, providing basic mechanical properties and durability;
[0066] Crosslinkers are used to enhance the thermal stability and mechanical strength of the topcoat, ensuring the integrity and durability of the coating under temperature changes;
[0067] Chromophores are thermosensitive compounds that undergo chemical structural changes at specific temperatures, causing color changes, which are used to provide visual feedback to indicate temperature changes;
[0068] Solvents and other auxiliary additives are used to adjust the viscosity, fluidity and drying time of the coating to facilitate the coating application and film formation process.
[0069] The present invention also includes a method for preparing an acrylic polyurethane topcoat, which is prepared as follows:
[0070] A heat-sensitive acrylic monomer is selected, and the monomer is mixed with a specific modified chromophore and an organic compound that can change the chemical structure when a predetermined temperature threshold is reached. Before mixing, the chromophore is surface treated or chemically modified to enhance its compatibility and stability with the acrylic monomer. The modification includes introducing appropriate functional groups on the surface of the chromophore to improve its dispersibility and reactivity in the monomer.
[0071] The mixing process is carried out in a high shear mixer, which can provide sufficient energy to break up the aggregates between the materials and ensure that the chromophore is evenly dispersed in the acrylic monomer. The stirring process is carried out at room temperature and lasts for about 30 minutes to 1 hour, depending on the desired degree of dispersion and the specific amount of materials used. Then, the polyurethane prepolymer is gradually added to the premixed mixture of heat-sensitive monomers and chromophores. The amount of polyurethane prepolymer added accounts for 40% to 50% of the total formulation. During the addition process, continuous stirring is carried out to maintain the uniformity of the mixture and avoid any precipitation or stratification of the components. The reaction mixture is then stirred for 2 hours at 60°C. This temperature and time are set to promote the cross-linking reaction between the polyurethane prepolymer and the heat-sensitive acrylic monomer, while allowing the chromophore to be fully integrated into the polymer network.
[0072] The crosslinking agent selected is an isocyanate compound. Isocyanate crosslinking agents can react with the hydroxyl groups in the polyurethane prepolymer to establish a strong three-dimensional network structure. The specific addition process is as follows:
[0073] Prepare a base mixture of heat-sensitive acrylic monomers and polyurethane prepolymers. Then, accurately weigh the isocyanate crosslinker according to the ratio of 3% to 5% of the total formula. Slowly and evenly add the crosslinker to the base mixture at room temperature. While adding the crosslinker, continue to stir with a high shear agitator to ensure that the crosslinker is evenly distributed throughout the base mixture to avoid any aggregated or unreacted crosslinker. Once the crosslinker is fully mixed, transfer the mixture to a curing oven preheated to 60°C, maintain the temperature and continue stirring for 2 hours to accelerate the crosslinking reaction and ensure temperature uniformity of the entire coating mixture during the curing process.
[0074] After the polyurethane prepolymer, heat-sensitive acrylic monomer and cross-linking agent are mixed uniformly in proportion, a predetermined proportion of solvent and leveling agent are gradually added to the mixture, and high-shear stirring equipment is used to mix the mixture for about 30 minutes to 1 hour to ensure that all ingredients are fully integrated without particles or aggregates;
[0075] The mixed coating is prepared at room temperature, and then the temperature of the curing environment is gradually increased to 80°C. The gradual temperature increase helps to control the curing speed and cross-linking density, and prevent uneven coating or stress accumulation caused by too rapid temperature increase. The entire temperature increase and maintenance process lasts for about 4 hours, which is enough to completely cross-link the polyurethane prepolymer to form a strong and durable coating. Before placing the coating in the curing environment, the mixture is treated in a high-speed centrifuge to remove unreacted monomers and any bubbles formed during the mixing process. The centrifugal treatment is carried out at a speed of several thousand to ten thousand revolutions per minute for several minutes, effectively bringing the bubbles and any suspended impurities to the top of the container so that they can be removed, ensuring the density and smoothness of the coating, reducing the need for subsequent processing, and improving the overall quality of the coating.
[0076] After high-speed centrifugation, set the UV lamp intensity to 500 mW / cm 2 The irradiation time is 5 minutes. The ultraviolet curing quickly activates the photoinitiator in the coating, accelerates the cross-linking reaction, and greatly shortens the curing time.
[0077] In the case of additional optimization of the cross-linking reaction, infrared heating is used to provide deeper heat penetration, especially for thicker coatings. Infrared heating ensures that the coating is heated evenly from the surface to the inside, avoiding the outer layer curing too quickly while the inner layer is still not fully reacted.
[0078] The technical features of the above embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0079] The principles and implementation methods of the present invention are described in this article using specific examples. The description of the above embodiments is only used to help understand the method and core idea of the present invention. At the same time, for those skilled in the art, according to the idea of the present invention, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as limiting the present invention.
Claims
1. An acrylic polyurethane topcoat, characterized in that: The topcoat comprises the following components in weight proportion: Heat sensitive acrylic monomer: 5-10% Polyurethane prepolymer: 40-50% Crosslinking agent: 3-5% Chromophore: 2-4% Organic solvents and other auxiliary additives: balance Wherein, the heat-sensitive acrylic monomer is a chromophore with thermochromic properties, which can change its color when a specific temperature threshold is reached; The polyurethane prepolymer is used to form the main structure of the coating and provide basic mechanical properties and durability; The cross-linking agent is used to enhance the thermal stability and mechanical strength of the topcoat, ensuring the integrity and durability of the coating under temperature changes; The chromophore is a thermosensitive compound that can undergo a chemical structural change at a specific temperature, thereby causing a color change, which is used to provide visual feedback to indicate temperature changes; The solvent and other auxiliary additives are used to adjust the viscosity, fluidity and drying time of the coating to facilitate the application and film-forming process of the coating.
2. The method for preparing an acrylic polyurethane topcoat according to claim 1, characterized in that: First, the heat-sensitive acrylic monomer was premixed with the modified chromophore in a high shear mixer to ensure that the chromophore was evenly dispersed in the monomer. Then, the polyurethane prepolymer was gradually added to the mixture and stirred at 60° C. for 2 hours to form a uniform reaction mixture.
3. The method for preparing an acrylic polyurethane topcoat according to claim 1, characterized in that: A specific proportion of crosslinking agent is added to the mixed heat-sensitive acrylic monomer and polyurethane prepolymer, wherein the crosslinking agent is selected from isocyanate to ensure the formation of a strong three-dimensional network structure in the subsequent curing process, thereby improving the mechanical properties and temperature resistance of the coating.
4. The method for preparing an acrylic polyurethane topcoat according to claim 1, characterized in that: The added organic solvent and other auxiliary additives include a leveling agent, the proportion of which in the final mixture is 10% of the total weight, and is used to adjust the fluidity and surface tension of the final coating to obtain ideal surface smoothness and glossiness.
5. The method for preparing an acrylic polyurethane topcoat according to claim 1, characterized in that: The curing process of the coating is carried out in an environment heated to 80°C and lasts for 4 hours. During this process, the temperature is gradually increased to control the curing speed and cross-linking density to ensure the uniformity of the coating and the final stable performance.
6. The method for preparing an acrylic polyurethane topcoat according to claim 1, characterized in that: Before the mixture is cured, it is centrifuged at high speed to remove unreacted monomers and formed bubbles. This step ensures the density and smoothness of the coating and reduces the need for subsequent treatment.
7. The method for preparing an acrylic polyurethane topcoat according to claim 1, characterized in that: UV curing technology is used, where the UV intensity is set to 500mW / cm 2 , the irradiation time is 5 minutes, which quickly cures the coating and improves production efficiency while ensuring that the physical and chemical properties of the coating meet the expected standards.
8. The method for preparing an acrylic polyurethane topcoat according to claim 1, characterized in that: By using infrared heating during the curing process, the cross-linking reaction of the coating is optimized. The use of infrared light penetrates deep into the coating and heats it evenly, avoiding excessive curing of the surface without sufficient reaction inside.
Citation Information
Patent Citations
UV-curable coating compositions and methods for using the same
CN104603217A
3D printing material with thermochromic property
CN105085833A
Production method of dual-curing solar glass panel capable of changing color along with scenes
CN110606668A
Infrared and ultraviolet combination curing machine
CN202263702U
Methods for obtaining colored or chromic substrates
US20190032277A1