Anti-fingerprint protective agent and use method thereof
By using a compounding technology for anti-fingerprint protectants, the problem of fingerprints easily remaining on the vacuum coating layer of automotive interior parts has been solved, improving its anti-fingerprint, wear-resistant, and corrosion-resistant properties, and extending its service life.
Patent Information
- Application Number
- CN202410975179.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-19
AI Technical Summary
The vacuum coating layer on existing automotive interior parts is prone to leaving fingerprints that are difficult to remove, affecting the user experience, and it lacks wear resistance and corrosion resistance.
An anti-fingerprint protective agent is used, which forms a dense and smooth anti-fingerprint protective film by compounding polytetrafluoroethylene, terpene phenol resin and sodium sulfide, enhancing the bonding strength and uniformity. Combining the adhesive properties of terpene phenol resin and the solubility properties of sodium sulfide, the anti-fingerprint, wear resistance and corrosion resistance are improved.
It effectively improves the fingerprint resistance, wear resistance, and corrosion resistance of automotive interior parts, extending their service life.
Smart Images

Figure BDA0004954318190000071 
Figure BDA0004954318190000081
Abstract
Description
Technical Field
[0001] The present invention relates to the field of surface treatment, and more particularly to an anti-fingerprint protective agent and a method for using the same. Background Art
[0002] As a traditional surface treatment technology, electroplating plays an important role in my country's industrial production. Electroplated parts are widely used in various industries due to their good corrosion resistance, aesthetics and practicality. In recent years, with the continuous development of science and technology, electroplating technology has also been continuously improved, and the appearance surface quality of automotive interior parts has also been significantly improved.
[0003] Most of the existing automotive interior products use a vacuum coating layer as their outermost layer, which not only makes it easy to obtain a variety of colors, but also the wear resistance of the vacuum coating layer is better than that of the electroplated chrome layer. Therefore, this technology is widely used. However, since the metal particles in the vacuum coating layer are very small, and the film layer is not dense and has many holes, when people hold the product with their hands, the sweat on their hands can easily adhere to the product, leaving fingerprints, and the fingerprints are not easy to clean, affecting the user experience. Summary of the invention
[0004] In order to effectively improve the anti-fingerprint property and service life of existing automobile interior decoration parts, the present application provides an anti-fingerprint protective agent and a method for using the same.
[0005] In the first aspect, the present application provides an anti-fingerprint protective agent, which adopts the following technical solution: An anti-fingerprint protective agent is made from the following raw material components in parts by weight: Nickel sulfate: 7 to 14 parts; Nickel chloride: 3 to 7 parts; Ferrous sulfate: 1.6 to 2.2 parts; Polytetrafluoroethylene: 11 to 14 parts; Nonionic surfactant: 3 to 6 parts; Main brightener: 0.06-0.12 parts; Auxiliary light agent: 0.7-1.3 parts; Stabilizer: 1.5 to 2.3 parts; Terpene phenol resin: 1.5 to 3.5 parts; Sodium sulfide: 2.3 to 3.6 parts.
[0006] By adopting the above technical scheme, the compounding effect between polytetrafluoroethylene, terpene phenol resin and sodium sulfide is utilized to produce a further synergistic effect with nickel sulfate, nickel chloride and ferrous sulfate, thereby improving the uniformity of the anti-fingerprint agent on the surface of the substrate, and at the same time, the binding strength of the anti-fingerprint agent on the substrate of the automotive interior decoration can be improved, while maintaining the bright metallic appearance of the substrate, having good anti-fingerprint properties, corrosion resistance and wear resistance, thereby achieving the purpose of extending the service life of the automotive interior decoration; Among them, by utilizing the extension and adhesion properties of terpene phenol resin, the molecular chain of polytetrafluoroethylene can be effectively extended and firmly covered on the surface of the substrate, and the metal nickel and iron ions in the solution can be better extended and diffused, effectively improving the dispersion uniformity of the nickel and iron ions in the solution. At the same time, through the high molecular weight network structure formed by the terpene phenol resin in the solution, the nickel and iron ions in the solution are more firmly deposited on the molecular chain of polytetrafluoroethylene to form a film; at the same time, by utilizing the solubility characteristics of sodium sulfide in polar organic solvents, the metal nickel and iron in the solution can be When the ions are deposited on the molecular chain of polytetrafluoroethylene, sodium sulfide is used to effectively fill the gaps between the nickel and iron ions and the polytetrafluoroethylene molecular chain, thereby making the formed anti-fingerprint agent film layer more uniform, reducing the situation where the uniformity of the electroplating layer is affected by local excessive aggregation, and effectively coordinating with nickel sulfate, nickel chloride and ferrous sulfate through the compound of terpene phenol resin, sodium sulfide and polytetrafluoroethylene to form a dense and smooth anti-fingerprint protective film layer on the surface of the substrate, thereby achieving the purpose of enhancing the anti-fingerprint, wear resistance and corrosion resistance of the surface of the substrate of automotive interior parts.
[0007] Optionally, the viscosity of the terpene phenol resin is 600 mPa·s.
[0008] Optionally, the sodium sulfide is monoclinic sodium sulfide.
[0009] Optionally, the degree of polymerization of the polytetrafluoroethylene is 3500.
[0010] By adopting the above technical solution and selecting terpene phenol resin, sodium sulfide and polytetrafluoroethylene materials with specific parameters, the compounding effect of the three in the solution can be further optimized, so that an automotive interior material with better anti-fingerprint, wear resistance and corrosion resistance can be obtained on the surface of the substrate.
[0011] Optionally, the buffer is one or both of disodium hydrogen phosphate and sodium bicarbonate.
[0012] Optionally, the primary light agent is one or both of mercaptoethanol and thioglycolic acid.
[0013] By adopting the above technical solution and selecting specific buffer and main light agent materials, the pH value in the solution can be better balanced, the precipitation of metal ions can be inhibited, and the deposition stability of metal ions on the polytetrafluoroethylene molecular chain can be maintained, which is conducive to uniform deposition on the surface of the substrate to obtain an anti-fingerprint protective film layer with better performance, thereby effectively extending the service life of automotive interior materials.
[0014] Optionally, the terpene phenol resin is pretreated and modified, and the pretreatment modification step includes: adding aluminum silicate and aminomethyltrimethoxysilane to a solvent and mixing them evenly to obtain a mixed solution A, adding the terpene phenol resin to be pretreated and modified to the mixed solution A to form a mixed solution B, heating the mixture to react, and then adding polyamide fiber to the mixed solution B to form a mixed solution C, stirring at a constant temperature, and obtaining a pretreated terpene phenol resin mixed solution after the reaction is completed.
[0015] By adopting the above technical scheme, the active hydroxyl or aluminum oxide group on the surface of aluminum silicate reacts with the hydroxyl, carboxyl and other functional groups in the terpene phenol resin to form a covalent bond or a coordination bond, thereby improving the surface characteristics of the terpene phenol resin molecular chain, so that the terpene phenol resin forms a uniform covering layer on the surface of aluminum silicate, thereby increasing its dispersibility and stability in the system. In addition, the ductility of the terpene phenol resin is improved by using polyamide fiber, and the terpene phenol resin can better produce a compounding effect with polytetrafluoroethylene and sodium sulfide, so that the terpene phenol resin can better adhere to the substrate and polytetrafluoroethylene, thereby further enhancing the adsorption effect between the metal nickel and iron ions in the solution and the polytetrafluoroethylene molecular chain, so as to further improve the anti-fingerprint, wear resistance and corrosion resistance of the anti-fingerprint protective film layer.
[0016] Optionally, the molar concentration of the aluminum silicate in the solvent is 0.45-0.6 mol / L, the molar concentration of the aminomethyltrimethoxysilane in the solvent is 0.3-0.5 mol / L, and the weight ratio of the polyamide fiber to the terpene phenol resin is 1.5:1.
[0017] Optionally, the degree of polymerization of the polyamide fiber is 850.
[0018] By adopting the above technical scheme, adjusting aluminum silicate to a suitable molar concentration or selecting polyamide fibers with a suitable degree of polymerization, the two can better interact with the molecular chain surface of the terpene phenol resin, improve the compatibility of the molecular chain surface of the terpene phenol resin with polytetrafluoroethylene and sodium sulfide substances in the solution, and enhance the dispersibility of sodium sulfide, so that sodium sulfide can be better filled in the gap between metal nickel, iron ions and polytetrafluoroethylene molecular chains, thereby improving and better enhancing the deposition stability of metal nickel and iron ions on the molecular chain surface of polytetrafluoroethylene in the solution.
[0019] In the second aspect, the present application provides a method for using an anti-fingerprint protective agent using the following technical solution: A method for using an anti-fingerprint protective agent comprises the following steps: The anti-fingerprint protective agent is pre-formulated according to the weight ratio; The surface treated substrate is immersed in the pre-configured anti-fingerprint protective agent, taken out, left to stand and baked to form an anti-fingerprint film layer on the substrate.
[0020] By adopting the above technical scheme, the terpene phenol resin, sodium sulfide and polytetrafluoroethylene can be compounded to form an anti-fingerprint protective agent which is evenly and stably combined with the surface of the substrate, so that the metal nickel and iron ions in the anti-fingerprint protective agent can be evenly dispersed on the polytetrafluoroethylene molecular chain, thereby effectively improving the coverage stability of the anti-fingerprint protective agent on the surface of the substrate.
[0021] In summary, this application has the following beneficial effects: 1. The present application utilizes the compounding effect between polytetrafluoroethylene, terpene phenol resin and sodium sulfide to produce a further synergistic effect with nickel sulfate, nickel chloride and ferrous sulfate, thereby improving the uniformity of the anti-fingerprint agent on the surface of the substrate, and at the same time improving the binding strength of the anti-fingerprint agent on the substrate of the automotive interior decoration, while maintaining the bright metallic appearance of the substrate while having good anti-fingerprint, corrosion resistance and wear resistance, thereby achieving the purpose of extending the service life of the automotive interior decoration; 2. The present application reacts the active hydroxyl or aluminum oxide group on the surface of aluminum silicate with the hydroxyl, carboxyl and other functional groups in the terpene phenol resin to form a covalent bond. The surface characteristics of the terpene phenol resin molecular chain are improved by forming a bond or coordination bond, so that the terpene phenol resin forms a uniform covering layer on the surface of aluminum silicate, thereby increasing its dispersibility and stability in the system. In addition, the ductility of the terpene phenol resin is improved by using polyamide fiber, and the terpene phenol resin can be better compounded with polytetrafluoroethylene and sodium sulfide, so that the terpene phenol resin can better adhere to the substrate and polytetrafluoroethylene, thereby further enhancing the adsorption effect between the metal nickel and iron ions in the solution and the polytetrafluoroethylene molecular chain, so as to further improve the anti-fingerprint, wear resistance and corrosion resistance of the anti-fingerprint protective film layer. DETAILED DESCRIPTION
[0022] The present application is further described in detail below in combination with preparation examples, embodiments, comparative examples and application examples.
[0023] Preparation Example 1 Preparation method of pretreated modified terpene phenol resin: 0.92 kg of aluminum silicate and 0.6 kg of aminomethyltrimethoxysilane were weighed according to the weight ratio and added into 10 L of 95% ethanol solvent, the temperature was raised to 60° C., and the mixture was stirred and mixed to obtain a mixed solution A; Weigh 0.35 kg of terpene phenol resin by weight and add it to mixed solution A, raise the temperature to 200° C., and stir and mix to obtain mixed solution B; 0.7 kg of polyamide fiber was weighed according to the weight ratio and added to the mixed solution B. The mixture was heated to 240° C. and stirred. After the reaction was completed, a pretreated terpene phenol resin mixed solution was obtained.
[0024] Preparation Example 2 Preparation method of pretreated modified terpene phenol resin: 0.84 kg of aluminum silicate and 0.3 kg of aminomethyltrimethoxysilane were weighed according to the weight ratio and added into 10 L of 95% ethanol solvent, the temperature was raised to 60° C., and the mixture was stirred and mixed to obtain a mixed solution A; Weigh 0.35 kg of terpene phenol resin by weight and add it to mixed solution A, raise the temperature to 200° C., and stir and mix to obtain mixed solution B; 0.525 kg of polyamide fiber was weighed according to the weight ratio and added to the mixed solution B. The temperature was raised to 240° C. and stirred. After the reaction was completed, a pretreated terpene phenol resin mixed solution was obtained.
[0025] Preparation Example 3 Preparation method of pretreated modified terpene phenol resin: 0.63 kg of aluminum silicate and 0.5 kg of aminomethyltrimethoxysilane were weighed according to the weight ratio and added into 10 L of 95% ethanol solvent, the temperature was raised to 60° C., and the mixture was stirred and mixed to obtain a mixed solution A; Weigh 0.35 kg of terpene phenol resin by weight and add it to mixed solution A, raise the temperature to 200° C., and stir and mix to obtain mixed solution B; 0.525 kg of polyamide fiber was weighed according to the weight ratio and added to the mixed solution B. The temperature was raised to 240° C. and stirred. After the reaction was completed, a pretreated terpene phenol resin mixed solution was obtained.
[0026] Example 1 An anti-fingerprint protective agent is prepared by the following steps: Step 1): 1.4 kg of nickel sulfate, 0.3 kg of nickel chloride and 0.16 kg of ferrous sulfate were weighed according to weight ratio and added into 10 L of deionized water, and stirred to mix well to form solution 1; Step 2): 1.1 kg of polytetrafluoroethylene, 0.15 kg of terpene phenol resin, 0.23 kg of sodium sulfide and 0.6 kg of fatty alcohol polyoxyethylene ether were weighed and added to the solvent according to the weight ratio, and the temperature was raised to 200° C. and stirred at a constant temperature to form a solution 2 after mixing evenly; Step 3): After the solution 1 and the solution 2 are stirred and mixed evenly, 0.012 kg of mercaptoethanol, 0.07 kg of sodium bicarbonate and 0.15 kg of sodium hydroxide are added according to the weight ratio, and then filtered through a 300-mesh filter screen, and after standing, an anti-fingerprint protective agent is prepared.
[0027] The viscosity of the terpene phenol resin is 800 mPa·s, the sodium sulfide is cubic sodium sulfide, and the degree of polymerization of polytetrafluoroethylene is 2500.
[0028] Example 2 Step 1): 0.7 kg of nickel sulfate, 0.7 kg of nickel chloride and 0.22 kg of ferrous sulfate were weighed according to weight ratio and added into 10 L of deionized water, and stirred to mix well to form solution 1; Step 2): 1.4 kg of polytetrafluoroethylene, 0.35 kg of terpene phenol resin, 0.36 kg of sodium sulfide and 0.3 kg of fatty alcohol polyoxyethylene ether were weighed and added to the solvent according to the weight ratio, and the temperature was raised to 200° C. and stirred at a constant temperature to form a solution 2 after mixing evenly; Step 3): After the solution 1 and the solution 2 are stirred and mixed evenly, 0.006 kg of mercaptoethanol, 0.13 kg of sodium bicarbonate and 0.35 kg of sodium hydroxide are added according to the weight ratio, and then filtered through a 300-mesh filter screen, and after standing, an anti-fingerprint protective agent is prepared.
[0029] The viscosity of the terpene phenol resin is 800 mPa·s, the sodium sulfide is cubic sodium sulfide, and the degree of polymerization of polytetrafluoroethylene is 2500.
[0030] Example 3 An anti-fingerprint protective agent, which is different from Example 2 in that the viscosity of the terpene phenol resin is 600 mPa·s.
[0031] Example 4 An anti-fingerprint protective agent, which is different from Example 2 in that the sodium sulfide is monoclinic sodium sulfide.
[0032] Example 5 An anti-fingerprint protective agent, which is different from Example 3 in that the degree of polymerization of polytetrafluoroethylene is 3500.
[0033] Example 6 An anti-fingerprint protective agent, which is different from Example 5 in that mercaptoethanol is replaced by thioglycolic acid.
[0034] Example 7 An anti-fingerprint protective agent, which is different from Example 5 in that mercaptoethanol is replaced by mercaptoethanol and thioglycolic acid, wherein mercaptoethanol and thioglycolic acid are used in a ratio of 1:1.
[0035] Example 8 An anti-fingerprint protective agent, which is different from Example 5 in that sodium bicarbonate is replaced by disodium hydrogen phosphate.
[0036] Example 9 An anti-fingerprint protective agent, which is different from Example 5 in that sodium bicarbonate is replaced by disodium hydrogen phosphate and sodium bicarbonate, wherein the disodium hydrogen phosphate and sodium bicarbonate are used in a ratio of 1:1.
[0037] Example 10 An anti-fingerprint protective agent, which is different from Example 5 in that the terpene phenol resin is the pre-treated modified terpene phenol resin mixed solution obtained in Preparation Example 1.
[0038] Embodiment 11 An anti-fingerprint protective agent, which is different from Example 5 in that the terpene phenol resin is the pre-treated modified terpene phenol resin mixed solution obtained in Preparation Example 2.
[0039] Example 12 An anti-fingerprint protective agent, which is different from Example 5 in that the terpene phenol resin is the pre-treated modified terpene phenol resin mixed liquid obtained in Preparation Example 3.
[0040] Comparative Example 1 The difference between this comparative example and Example 1 is that the terpene phenol resin is replaced by an equal amount of water.
[0041] Comparative Example 2 The difference between this comparative example and Example 1 is that sodium sulfide is replaced by an equal amount of water.
[0042] Comparative Example 3 The difference between this comparative example and Example 1 is that the terpene phenol resin and sodium sulfide are both replaced by an equal amount of water.
[0043] Application Example 1-15 A method for using an anti-fingerprint protective agent: soak the substrate that has been subjected to surface washing and degreasing treatment in the anti-fingerprint protective agent prepared in Examples 1-12 and Comparative Examples 1-3 for 30 seconds, take it out and let it stand, then bake the substrate at 60° C. for 30 minutes, and finally form an anti-fingerprint film layer on the surface of the substrate. The substrate can be a metal interior part such as aluminum alloy, stainless steel or magnesium alloy of an automobile.
[0044] Performance testing 1) Thickness test The substrate cut volume in Application Example 1-15 is 5 cm 3 The samples were placed in an ellipsometer for thickness measurement. The smaller the change in the thickness of the anti-fingerprint film at multiple positions in the sample, the better the uniformity of the anti-fingerprint film formed on the surface of the substrate. Among them, if the thickness distribution of the anti-fingerprint film is uniform, it is recorded as "excellent", and if the thickness distribution is uneven, it is recorded as "poor".
[0045] 2) Wear resistance test The substrate cut volume in Application Example 1-15 is 5 cm 3 The sample is rubbed at a speed of 10 mm / s under an initial load of 1 N force using a MCJ-01 scratch resistance tester (provided by Jinan Grete Testing Instrument Co., Ltd.); and the force is increased by 1 N every 1 second until scratches appear on the surface of the test piece, and the needle load value (N) at this time is recorded. The larger the needle load value, the better the wear resistance of the anti-fingerprint film layer.
[0046] 3) Corrosion resistance test The substrate cut volume in Application Example 1-15 is 5 cm 3 For the sample, the thickness at multiple positions was measured by ellipsometer, and the average value was taken and recorded as a1. The sample was then immersed in 8% dilute sulfuric acid for 24 hours. After being taken out, the thickness at multiple positions was measured by ellipsometer, and the average value was taken and recorded as a2. The thickness difference (nm) before and after immersion of multiple samples a1-a2 was calculated. The smaller the thickness difference, the better the corrosion resistance and anti-fingerprint properties of the anti-fingerprint film layer formed on the surface of the substrate.
[0047] Table 1-Summary of test data for application examples 1-15 According to the comparison of the test data of Application Example 1 and Application Example 15 in Table 1, the anti-fingerprint film layer of the substrate of the automotive interior parts prepared according to the technical solution of the present application is significantly improved in terms of wear resistance, corrosion resistance and anti-fingerprint performance compared to the anti-fingerprint film layer of the substrate of the existing automotive interior parts without the addition of terpene phenol resin, sodium sulfide and polytetrafluoroethylene. In addition, while effectively optimizing the various properties of the existing automotive metal interior parts substrate without the need for high temperature, the thickness uniformity of the anti-fingerprint film layer of the substrate can also be effectively improved, thereby achieving the purpose of extending the service life of the automotive interior substrate of the present application; In addition, by comparing the test data of Application Example 1 and Application Examples 13-15, it can be seen that if the synergistic effect of terpene phenol resin, sodium sulfide and polytetrafluoroethylene is destroyed in the system, the wear resistance, corrosion resistance and anti-fingerprint performance of the anti-fingerprint film layer of the prepared automotive metal interior parts substrate and the uniformity of the anti-fingerprint film layer will be reduced to varying degrees, indicating that the three are indispensable in the anti-fingerprint protective agent of the technical solution of the present application. It is known that the prerequisite for improving the performance of the anti-fingerprint film layer of the automotive metal interior parts substrate of the present application is the synergistic cooperation of the three to obtain a more effective synergistic effect on the anti-fingerprint film layer of the automotive metal interior parts substrate.
[0048] According to the comparison of the experimental data of Application Examples 1-2 in Table 1, it can be seen that when the inventor controls the weight ratio of terpene phenol resin, sodium sulfide and polytetrafluoroethylene in the electroplating solution, the wear resistance, corrosion resistance and anti-fingerprint performance of the anti-fingerprint film layer of the silicon chip automotive metal interior parts substrate of the present application can be better improved, thereby achieving the purpose of further improving the service life of the automotive metal interior parts substrate of the present application.
[0049] According to the comparison of the test data of Application Examples 2-5 in Table 1, it can be seen that when the inventor selects terpene phenol resin, sodium sulfide and polytetrafluoroethylene with specific material properties or structural forms for addition, the friction resistance of the anti-fingerprint film layer of the automotive metal interior parts substrate of the present application can be further enhanced, and at the same time, the thickness difference before and after corrosion can be more effectively reduced, thereby more effectively improving the service life and application range of the automotive metal interior parts substrate of the present application.
[0050] According to the comparison of the test data of Application Examples 5-9 in Table 1, it can be seen that when the inventors select specific types of primary light agents and stabilizers for addition, it can be clearly seen that the anti-fingerprint film layer of the automotive metal interior parts substrate of the present application is enhanced to a greater extent in terms of wear resistance, corrosion resistance and anti-fingerprint performance, thereby enabling the automotive metal interior parts substrate prepared by the present application to be further improved in terms of service life and application scope, and has great economic value.
[0051] According to the comparison of the test data of Application Examples 5 and 10 in Table 1, it can be seen that when the inventors choose to add the pre-treated modified terpene phenol resin, the anti-fingerprint film layer of the automotive metal interior substrate in the technical solution of the present application is greatly enhanced in wear resistance, corrosion resistance and anti-fingerprint performance, indicating that the surface characteristics of the modified terpene phenol resin molecular chain are effectively improved, so that the terpene phenol resin can better produce a synergistic effect with polytetrafluoroethylene and sodium sulfide.
[0052] According to the comparison of the test data of application examples 5, 10-12 in Table 1, it can be seen that when the inventor selects aluminum silicate and aminomethyltrimethoxysilane with a specific molar concentration and polyamide fiber with a specific weight ratio to limit the change of the pretreatment conditions, the wear resistance of the anti-fingerprint film layer of the automotive metal interior substrate of the present application can be enhanced to a greater extent, and the corrosion resistance and anti-fingerprint performance of the anti-fingerprint film layer of the automotive metal interior substrate can be better improved, so that the automotive metal interior substrate of the present application can adapt to the use under more working conditions, so as to achieve the effect of improving the service life and application range of existing automotive metal interior parts.
[0053] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. An anti-fingerprint protective agent, It is characterized in that The invention is made of the following raw material components in parts by weight: Nickel sulfate: 7 to 14 parts; Nickel chloride: 3 to 7 parts; Ferrous sulfate: 1.6 to 2.2 parts; Polytetrafluoroethylene: 11 to 14 parts; Nonionic surfactant: 3 to 6 parts; Main brightener: 0.06~0.12 parts; Auxiliary light agent: 0.7~1.3 parts; Stabilizer: 1.5~2.3 parts; Terpene phenol resin: 1.5 to 3.5 parts; Sodium sulfide: 2.3~3.6 parts.
2. An anti-fingerprint protective agent according to claim 1, It is characterized in that The viscosity of the terpene phenol resin is 600 mPa·s.
3. An anti-fingerprint protective agent according to claim 1, It is characterized in that The sodium sulfide is monoclinic sodium sulfide.
4. An anti-fingerprint protective agent according to any one of claims 2-3, It is characterized in that The polymerization degree of the polytetrafluoroethylene is 3500.
5. An anti-fingerprint protective agent according to claim 4, It is characterized in that The primary light agent is one or both of mercaptoethanol and thioglycolic acid.
6. The anti-fingerprint protective agent according to claim 4, It is characterized in that The auxiliary light agent is one or both of disodium hydrogen phosphate and sodium bicarbonate.
7. An anti-fingerprint protective agent according to claim 4, It is characterized in that The terpene phenol resin is pretreated and modified, and the pretreatment and modification steps include: adding aluminum silicate and aminomethyltrimethoxysilane to a solvent, heating and stirring, and mixing evenly to obtain a mixed solution A, adding the terpene phenol resin to be pretreated and modified to the mixed solution A to form a mixed solution B, heating and reacting, and then adding polyamide fiber to the mixed solution B to form a mixed solution C, heating and stirring, and obtaining a pretreated terpene phenol resin mixed solution after the reaction is completed.
8. An anti-fingerprint protective agent according to claim 7, It is characterized in that The molar concentration of the aluminum silicate in the solvent is 0.45-0.6 mol / L, the molar concentration of the aminomethyltrimethoxysilane in the solvent is 0.3-0.5 mol / L, and the weight ratio of the polyamide fiber to the terpene phenol resin is 1.5:
1.
9. The anti-fingerprint protective agent according to claim 7, It is characterized in that The degree of polymerization of the polyamide fiber is 850.
10. A method for using an anti-fingerprint protective agent according to any one of claims 1 to 9, It is characterized in that The following steps are involved: The anti-fingerprint protective agent is pre-formulated according to the weight ratio; The surface treated substrate is immersed in the pre-configured anti-fingerprint protective agent, taken out, left to stand and baked to form an anti-fingerprint film layer on the substrate.
Citation Information
Patent Citations
Anti-fingerprint agent, and method and product applying the same to conduct surface treatment
CN103160174A
Anti-fingerprint coating composition and preparation method thereof as well as anti-fingerprint coating and preparation method thereof
CN108676442A
Surface treatment composition for zinc alloy plated steel sheet, zinc alloy plated steel sheet surface-treated using same and method for manufacturing same
WO2024107018A1