Negative oxygen ion ecological coating and preparation method thereof

By using paint raw materials and preparation methods with specific ratios, the continuous release amount and stability of negative oxygen ions are improved, and the problems of low release amount and poor moisture-proof and mildew-proof performance are solved, and efficient air purification and environmental protection are achieved. Production of coatings.

CN118931292APending Publication Date: 2024-11-12JIANGXI FENGLONG TEXTILE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411141304.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing negative oxygen ion coatings have low negative ions released, and are not moisture-proof or mildew-proof. They cannot continuously and stably release negative ions, affecting the air purification effect.

Method used

Negative oxygen ion ecological coatings prepared from silicone modified acrylic resin, silicone modified polyester resin, negative oxygen ion essence, ultra-fine light calcium, activated carbon powder and other raw materials are improved through specific mixing and ultrasonic treatment methods. Negative ion release amount and stability, and anti-mold agents and anti-bacterial agents are added to enhance waterproof and anti-bacterial properties.

Benefits of technology

The continuous and stable release of negative oxygen ions is achieved, the air purification effect is improved, the production cost is reduced, and good waterproof and mildew-proof performance is shown under different air humidity conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005000882500000131
    Figure BDA0005000882500000131
  • Figure BDA0005000882500000132
    Figure BDA0005000882500000132
  • Figure BDA0005000882500000141
    Figure BDA0005000882500000141
Patent Text Reader

Abstract

The invention provides a negative oxygen ion ecological coating and a preparation method thereof, and belongs to the field of coatings. The negative oxygen ion ecological coating is prepared from the following raw materials: organic silicon modified acrylic resin, organic silicon modified polyester resin, negative oxygen ion essence, superfine light calcium carbonate, a solvent, activated carbon powder, a curing agent, a dispersing agent, a defoaming agent, a wetting agent, a thickening agent, a mildew preventive, a flatting agent, an antibacterial agent, a coalescing agent and an anti-settling agent. The coating is green and environmentally friendly, the preparation process is simple, the production cost is reduced, and the prepared coating is high in negative oxygen ion continuous release amount, good in waterproof performance, small in influence of air humidity change and stable in negative oxygen ion continuous release amount.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of coatings, and in particular to a negative oxygen ion ecological coating and a preparation method thereof. Background Art

[0002] With the improvement of indoor air quality standards at home and abroad and the enhancement of people's environmental awareness, ecological and environmentally friendly multifunctional coatings have received more and more attention. Negative oxygen ion coatings are widely used in daily life due to their powerful effects. For example, negative oxygen ion coatings have a certain negative charge in negative ions, so when negative ions encounter dust in the air, positive and negative charges gather, and the dust will fall on the ground after increasing its weight, thereby achieving the effect of purifying the air; the (O2) activity of negative oxygen ions is very large, and formaldehyde (CH2O) can be actively captured, and then it will be forcibly decomposed. Negative oxygen ions also have powerful sterilization and disinfection functions. If negative oxygen ion coatings are to continuously release negative ions, it is necessary that when the moisture in the air contacts the coating, the moisture can be electrolyzed to generate negative ions, and the water molecules in the air react with the coating after the reaction, and negative ions can be continuously released. Through this continuous accumulation, the indoor negative ion concentration reaches a relatively stable and high level. The existing negative oxygen ion coatings release low negative ions and are not moisture-proof or mildew-proof. To this end, the present invention proposes a negative oxygen ion ecological coating and a preparation method thereof to solve the defects and deficiencies of the prior art. Summary of the invention

[0003] In view of the above-mentioned problems, the present invention proposes a negative oxygen ion ecological paint.

[0004] In order to achieve the above-mentioned purpose, the present invention adopts the following technical solutions:

[0005] A negative oxygen ion ecological paint, the negative oxygen ion ecological paint is prepared from the following raw materials in parts by weight:

[0006] 70-90 parts of silicone modified acrylic resin;

[0007] 40-60 parts of silicone modified polyester resin;

[0008] 10-15 portions of negative oxygen ion essence;

[0009] 5-10 portions of ultrafine light calcium;

[0010] 30-55 parts of solvent;

[0011] 3-10 parts of activated carbon powder;

[0012] Curing agent 0.5-1 part;

[0013] Dispersant 0.5-1 part;

[0014] Defoaming agent 0.1-0.5 parts;

[0015] Wetting agent 0.1-0.5 parts;

[0016] Thickener 0.1-0.5 parts;

[0017] 0.1-0.3 parts of mildew inhibitor;

[0018] Leveling agent 0.1-0.5 parts;

[0019] 1-2.5 parts of antibacterial agent;

[0020] Film-forming aid 0.4-0.9 parts;

[0021] Anti-settling agent 0.1-0.5 parts.

[0022] Preferably, the negative oxygen ion ecological paint is prepared from the following raw materials in parts by weight:

[0023] 75-85 parts of silicone modified acrylic resin;

[0024] 45-55 parts of silicone modified polyester resin;

[0025] Negative oxygen ion essence 11-13 parts;

[0026] 6-8 portions of ultrafine light calcium;

[0027] 35-50 parts of solvent;

[0028] 5-7 parts of activated carbon powder;

[0029] Curing agent 0.6-0.8 parts;

[0030] Dispersant 0.6-0.8 parts;

[0031] Defoaming agent 0.2-0.4 parts;

[0032] Wetting agent 0.2-0.4 parts;

[0033] Thickener 0.2-0.4 parts;

[0034] 0.1-0.2 parts of mildew inhibitor;

[0035] Leveling agent 0.2-0.4 parts;

[0036] Antibacterial agent 1.4-2 parts;

[0037] Film-forming aid 0.5-0.8 parts;

[0038] Anti-settling agent 0.2-0.4 parts.

[0039] Preferably, the negative oxygen ion ecological paint is prepared from the following raw materials in parts by weight:

[0040] 80 parts of silicone modified acrylic resin;

[0041] 50 parts of silicone modified polyester resin;

[0042] Negative oxygen ion essence 12 servings;

[0043] 7 parts of ultra-fine light calcium;

[0044] 42 parts of solvent;

[0045] 6.5 parts of activated carbon powder;

[0046] 0.7 parts of curing agent;

[0047] Dispersant 0.7 parts;

[0048] 0.3 parts of defoaming agent;

[0049] Wetting agent 0.3 parts;

[0050] Thickener 0.3 parts;

[0051] 0.1-0.2 parts of mildew inhibitor;

[0052] 0.3 parts of leveling agent;

[0053] 1.7 parts of antibacterial agent;

[0054] 0.7 parts of film-forming aid;

[0055] 0.3 parts of anti-settling agent.

[0056] Preferably, the solvent is diethylene glycol butyl ether;

[0057] The curing agent is a water-dispersible polyisocyanate;

[0058] The dispersant is SN-5040 or sodium salt of polycarboxylate or sodium polyacrylate or sodium lauryl sulfate; the defoamer is fatty acid amide or polysiloxane copolymer;

[0059] The wetting agent is polyether-modified siloxane;

[0060] The thickener is a polyurethane thickener;

[0061] The mildew preventer is 361 mildew preventer;

[0062] The leveling agent is fluorocarbon leveling agent or acrylic acid or MOK-2050;

[0063] The antimicrobial agent is a nanosilver colloidal solution;

[0064] The film-forming aid is ester alcohol dodeca or dipropylene glycol methyl ether or tripropylene glycol butyl ether;

[0065] The anti-settling agent is bentonite.

[0066] Preferably, the preparation method specifically comprises the following steps:

[0067] (1) mixing an organosilicon-modified acrylic resin and an organosilicon-modified polyester resin in a mixer, and controlling the mixing temperature at 45-50° C.;

[0068] (2) adding ultrafine light calcium, solvent, activated carbon powder, curing agent, dispersant, defoamer, wetting agent, thickener, mildewproof agent, leveling agent, antibacterial agent, film-forming aid, and anti-settling agent, and mixing and stirring in a high-speed stirrer at 800-1000 rpm;

[0069] (3) Finally, add the negative oxygen ion essence, apply ultrasonic treatment for 10-15 minutes, and then mix and stir in a high-speed mixer to obtain the negative oxygen ion ecological paint.

[0070] Preferably, the negative oxygen ion essence is prepared from the following raw materials in percentage by mass:

[0071] 15-20% of nano-tourmaline particles, 15-20% of ultrafine diatomaceous earth particles, 0.1-1% of dispersant, 0.1-0.5% of anionic surfactant, and the balance of plant extract.

[0072] Preferably, the negative oxygen ion essence is prepared from the following raw materials in percentage by mass:

[0073] 16.5% of nano-tourmaline particles, 18% of ultrafine diatomaceous earth particles, 0.4% of dispersant, 0.3% of anionic surfactant, and the balance of plant extract.

[0074] Preferably, the preparation steps of the negative oxygen ion essence include:

[0075] Mix nano tourmaline particles, ultrafine diatomaceous earth particles, dispersant, anionic surfactant and plant extract, mix and stir in a high-speed blender, control the stirring speed at 1200-1500rpm, and after the stirring is completed, the negative oxygen ion essence is obtained.

[0076] Preferably, the method for preparing the plant extract comprises the following steps:

[0077] (1) crushing and mixing ivy, mint, and aloe, freezing and crushing, pulverizing in a high-speed crusher, and further grinding in an ultrafine grinder, then washing with 10-15° C. purified water, mixing and dispersing in a high-speed stirrer at 1200-1500 rpm, removing the upper floating matter, standing at a constant temperature of 10-15° C. for 10-12 hours, and filtering to obtain a filtrate and a filter residue;

[0078] (2) drying the filter residue at 55-60° C. for 2-3 hours, and further grinding the powder obtained after drying, and passing it through a 500-mesh sieve to obtain a plant extract powder;

[0079] (3) The filtrate is concentrated to half of its original volume, and then a surfactant and the above-mentioned plant extract powder are added, mixed and dispersed in a high-speed stirrer at 1000-1200 rpm, and the plant extract is obtained by discharging.

[0080] Due to the adoption of the above technical scheme, the beneficial effects of the present invention are as follows: the coating of the present invention is not only green and environmentally friendly, but also has a simple preparation process and reduces production costs. The prepared coating has a high sustained release of negative oxygen ions, good waterproof performance, is less affected by changes in air humidity, and has a stable sustained release of negative oxygen ions. DETAILED DESCRIPTION

[0081] To make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0082] Embodiment 1:

[0083] The negative oxygen ion ecological coating of this embodiment 1 is prepared from the following raw materials in parts by weight:

[0084] 80 parts of silicone modified acrylic resin; 50 parts of silicone modified polyester resin; 12 parts of negative oxygen ion essence; 7 parts of ultrafine light calcium; 42 parts of solvent; 6.5 parts of activated carbon powder; 0.7 parts of curing agent; 0.7 parts of dispersant; 0.3 parts of defoaming agent; 0.3 parts of wetting agent; 0.3 parts of thickener; 0.1-0.2 parts of mildewproof agent; 0.3 parts of leveling agent; 1.7 parts of antibacterial agent; 0.7 parts of film-forming aid; 0.3 parts of anti-settling agent.

[0085] Among them, the solvent is diethylene glycol butyl ether; the curing agent is water-dispersible polyisocyanate; the dispersant is polycarboxylic acid sodium salt and sodium polyacrylate; the defoaming agent is fatty acid amide; the wetting agent is polyether modified siloxane; the thickener is a polyurethane thickener; the mildewproof agent is 361 mildewproof agent; the leveling agent is fluorocarbon leveling agent; the antibacterial agent is nanosilver colloidal solution; the film-forming aid is ester alcohol twelve; and the anti-settling agent is bentonite.

[0086] The preparation method of the negative oxygen ion ecological coating specifically comprises the following steps:

[0087] (1) mixing an organosilicon-modified acrylic resin and an organosilicon-modified polyester resin in a mixer, and controlling the mixing temperature at 50° C.;

[0088] (2) adding ultrafine light calcium, solvent, activated carbon powder, curing agent, dispersant, defoamer, wetting agent, thickener, mildewproof agent, leveling agent, antibacterial agent, film-forming aid, and anti-settling agent, and mixing and stirring in a high-speed stirrer at 1000 rpm;

[0089] (3) Finally, negative oxygen ion essence is added, and ultrasonic treatment is applied for 15 minutes, and then mixed and stirred in a high-speed mixer to obtain negative oxygen ion ecological paint.

[0090] The negative oxygen ion essence is prepared from the following raw materials in percentage by mass:

[0091] 16.5% of nano-tourmaline particles, 18% of ultrafine diatomaceous earth particles, 0.4% of dispersant, 0.3% of anionic surfactant, and the balance of plant extract.

[0092] The preparation steps of negative oxygen ion essence include:

[0093] Mix nano tourmaline particles, ultrafine diatomaceous earth particles, dispersant, anionic surfactant and plant extract, mix and stir in a high-speed blender, control the stirring speed at 1300 rpm, and after the stirring is completed, the negative oxygen ion essence is obtained.

[0094] The method for preparing the plant extract specifically comprises the following steps:

[0095] (1) crushing and mixing ivy, mint, and aloe, freezing and crushing, pulverizing in a high-speed crusher, further grinding and refining in an ultrafine grinder, washing with 12° C. purified water, mixing and dispersing in a high-speed stirrer at 1300 rpm, removing the upper floating matter, standing at a constant temperature of 12° C. for 11 hours, filtering, and obtaining a filtrate and a filter residue;

[0096] (2) drying the filter residue at 60° C. for 2.5 h, and further grinding the powder obtained after drying, and passing it through a 500-mesh sieve to obtain a plant extract powder;

[0097] (3) The filtrate was concentrated to half of its original volume, and then a surfactant and the above-mentioned plant extract powder were added, and mixed and dispersed in a high-speed stirrer at 1200 rpm to obtain a plant extract solution.

[0098] Embodiment 2:

[0099] The negative oxygen ion ecological coating of this embodiment 2 is prepared from the following raw materials in parts by weight:

[0100] 90 parts of silicone modified acrylic resin; 60 parts of silicone modified polyester resin; 15 parts of negative oxygen ion essence; 10 parts of ultrafine light calcium; 55 parts of solvent; 10 parts of activated carbon powder; 1 part of curing agent; 1 part of dispersant; 0.5 parts of defoaming agent; 0.5 parts of wetting agent; 0.5 parts of thickener; 0.3 parts of mildewproof agent; 0.5 parts of leveling agent; 2.5 parts of antibacterial agent; 0.9 parts of film-forming aid; 0.5 parts of anti-settling agent.

[0101] Among them, the solvent is diethylene glycol butyl ether; the curing agent is water-dispersible polyisocyanate; the dispersing agent is SN-5040 and sodium dodecyl sulfate; the defoaming agent is fatty acid amide; the wetting agent is polyether modified siloxane; the thickener is a polyurethane thickener; the mildewproof agent is 361 mildewproof agent; the leveling agent is a fluorocarbon leveling agent; the antibacterial agent is nanosilver colloidal solution; the film-forming aid is tripropylene glycol butyl ether; and the anti-settling agent is bentonite.

[0102] The preparation method of the negative oxygen ion ecological coating specifically comprises the following steps:

[0103] (1) mixing an organosilicon-modified acrylic resin and an organosilicon-modified polyester resin in a mixer, and controlling the mixing temperature at 45° C.;

[0104] (2) adding ultrafine light calcium, solvent, activated carbon powder, curing agent, dispersant, defoamer, wetting agent, thickener, mildew preventer, leveling agent, antibacterial agent, film-forming aid, and anti-settling agent, and mixing and stirring in a high-speed stirrer at 800 rpm;

[0105] (3) Finally, negative oxygen ion essence is added, and ultrasonic treatment is applied for 10 minutes, and then mixed and stirred in a high-speed mixer to obtain negative oxygen ion ecological paint.

[0106] The negative oxygen ion essence is prepared from the following raw materials in percentage by mass:

[0107] 15% of nano-tourmaline particles, 15% of ultrafine diatomaceous earth particles, 0.1% of dispersant, 0.1% of anionic surfactant, and the balance of plant extract.

[0108] The preparation steps of negative oxygen ion essence include:

[0109] Mix nano tourmaline particles, ultrafine diatomaceous earth particles, dispersant, anionic surfactant and plant extract, mix and stir in a high-speed blender, control the stirring speed at 1200rpm, and after the stirring is completed, the negative oxygen ion essence is obtained.

[0110] The method for preparing the plant extract specifically comprises the following steps:

[0111] (1) crushing and mixing ivy, mint, and aloe, freezing and crushing, pulverizing in a high-speed crusher, further grinding and refining in an ultrafine grinder, washing with 10° C. purified water, mixing and dispersing in a high-speed stirrer at 1200 rpm, removing the upper floating matter, standing at a constant temperature of 10° C. for 10 hours, filtering, and obtaining a filtrate and a filter residue;

[0112] (2) drying the filter residue at 55° C. for 2 h, and further grinding the powder obtained after drying, and passing it through a 500-mesh sieve to obtain a plant extract powder;

[0113] (3) The filtrate was concentrated to half of its original volume, and then a surfactant and the above-mentioned plant extract powder were added, and mixed and dispersed in a high-speed stirrer at 1000 rpm to obtain a plant extract solution.

[0114] Embodiment 3:

[0115] The negative oxygen ion ecological coating of this embodiment 3 is prepared from the following raw materials in parts by weight:

[0116] 70 parts of silicone modified acrylic resin; 40 parts of silicone modified polyester resin; 10 parts of negative oxygen ion essence; 5 parts of ultrafine light calcium; 30 parts of solvent; 3 parts of activated carbon powder; 0.5 parts of curing agent; 0.5 parts of dispersant; 0.1 parts of defoaming agent; 0.1 parts of wetting agent; 0.1 parts of thickener; 0.1 parts of mildewproof agent; 0.1 parts of leveling agent; 1 part of antibacterial agent; 0.4 parts of film-forming aid; 0.1 parts of anti-settling agent.

[0117] Among them, the solvent is diethylene glycol butyl ether; the curing agent is water-dispersible polyisocyanate; the dispersant is sodium dodecyl sulfate; the defoaming agent is fatty acid amide; the wetting agent is polyether modified siloxane; the thickener is a polyurethane thickener; the mildewproof agent is 361 mildewproof agent; the leveling agent is fluorocarbon leveling agent and acrylic acid; the antibacterial agent is nanosilver colloidal solution; the film-forming aid is dipropylene glycol methyl ether; and the anti-settling agent is bentonite.

[0118] The preparation method of the negative oxygen ion ecological coating specifically comprises the following steps:

[0119] (1) mixing an organosilicon-modified acrylic resin and an organosilicon-modified polyester resin in a mixer, and controlling the mixing temperature at 45° C.;

[0120] (2) adding ultrafine light calcium, solvent, activated carbon powder, curing agent, dispersant, defoamer, wetting agent, thickener, mildew preventer, leveling agent, antibacterial agent, film-forming aid, and anti-settling agent, and mixing and stirring in a high-speed stirrer at 800 rpm;

[0121] (3) Finally, negative oxygen ion essence is added, and ultrasonic treatment is applied for 12 minutes, and then mixed and stirred in a high-speed mixer to obtain negative oxygen ion ecological paint.

[0122] The negative oxygen ion essence is prepared from the following raw materials in percentage by mass:

[0123] 20% of nano-tourmaline particles, 20% of ultrafine diatomaceous earth particles, 1% of dispersant, 0.5% of anionic surfactant, and the balance of plant extract.

[0124] The preparation steps of negative oxygen ion essence include:

[0125] Mix nano tourmaline particles, ultrafine diatomaceous earth particles, dispersant, anionic surfactant and plant extract, mix and stir in a high-speed blender, control the stirring speed at 1500rpm, and after the stirring is completed, the negative oxygen ion essence is obtained.

[0126] The method for preparing the plant extract specifically comprises the following steps:

[0127] (1) crushing and mixing ivy, mint, and aloe, freezing and crushing, pulverizing in a high-speed crusher, further grinding and refining in an ultrafine grinder, washing with 15° C. purified water, mixing and dispersing in a high-speed stirrer at 1300 rpm, removing the upper floating matter, standing at a constant temperature of 15° C. for 12 hours, filtering, and obtaining a filtrate and a filter residue;

[0128] (2) drying the filter residue at 60° C. for 3 h, and further grinding the powder obtained after drying, and passing it through a 500-mesh sieve to obtain a plant extract powder;

[0129] (3) The filtrate was concentrated to half of its original volume, and then a surfactant and the above-mentioned plant extract powder were added, and mixed and dispersed in a high-speed stirrer at 1200 rpm to obtain a plant extract solution.

[0130] Embodiment 4:

[0131] The negative oxygen ion ecological coating of this embodiment 4 is prepared from the following raw materials in parts by weight:

[0132] 85 parts of silicone modified acrylic resin; 55 parts of silicone modified polyester resin; 13 parts of negative oxygen ion essence; 8 parts of ultrafine light calcium; 50 parts of solvent; 7 parts of activated carbon powder; 0.8 parts of curing agent; 0.8 parts of dispersant; 0.4 parts of defoaming agent; 0.4 parts of wetting agent; 0.4 parts of thickener; 0.2 parts of mildewproof agent; 0.4 parts of leveling agent; 2 parts of antibacterial agent; 0.8 parts of film-forming aid; 0.4 parts of anti-settling agent.

[0133] Among them, the solvent is diethylene glycol butyl ether; the curing agent is water-dispersible polyisocyanate; the dispersant is sodium dodecyl sulfate; the defoaming agent is polysiloxane copolymer; the wetting agent is polyether modified siloxane; the thickener is a polyurethane thickener; the mildewproof agent is 361 mildewproof agent; the leveling agent is MOK-2050; the antibacterial agent is nanosilver colloidal solution; the film-forming aid is tripropylene glycol butyl ether; and the anti-settling agent is bentonite.

[0134] The preparation method of the negative oxygen ion ecological coating specifically comprises the following steps:

[0135] (1) mixing an organosilicon-modified acrylic resin and an organosilicon-modified polyester resin in a mixer, and controlling the mixing temperature at 47° C.;

[0136] (2) adding ultrafine light calcium, solvent, activated carbon powder, curing agent, dispersant, defoamer, wetting agent, thickener, mildew preventer, leveling agent, antibacterial agent, film-forming aid, and anti-settling agent, and mixing and stirring in a high-speed stirrer at 900 rpm;

[0137] (3) Finally, negative oxygen ion essence was added, and ultrasonic treatment was applied for 14 minutes, and then mixed and stirred in a high-speed mixer to obtain negative oxygen ion ecological paint.

[0138] The negative oxygen ion essence is prepared from the following raw materials in percentage by mass:

[0139] Nano tourmaline particles 19%, ultrafine diatomaceous earth particles 16%, dispersant 0.9%, anionic surfactant 0.4%, and plant extract as the balance.

[0140] The preparation steps of negative oxygen ion essence include:

[0141] Mix nano tourmaline particles, ultrafine diatomaceous earth particles, dispersant, anionic surfactant and plant extract, mix and stir in a high-speed blender, control the stirring speed at 1500rpm, and after the stirring is completed, the negative oxygen ion essence is obtained.

[0142] The method for preparing the plant extract specifically comprises the following steps:

[0143] (1) crushing and mixing ivy, mint, and aloe, freezing and crushing, pulverizing in a high-speed crusher, further grinding and refining in an ultrafine grinder, washing with 14° C. purified water, mixing and dispersing in a high-speed stirrer at 1400 rpm, removing the upper floating matter, standing at a constant temperature of 14° C. for 12 hours, filtering, and obtaining a filtrate and a filter residue;

[0144] (2) drying the filter residue at 55° C. for 3 h, and further grinding the powder obtained after drying, and passing it through a 500-mesh sieve to obtain a plant extract powder;

[0145] (3) The filtrate was concentrated to half of its original volume, and then a surfactant and the above-mentioned plant extract powder were added, and mixed and dispersed in a high-speed stirrer at 1200 rpm to obtain a plant extract solution.

[0146] Embodiment 5:

[0147] The negative oxygen ion ecological coating of this embodiment 5 is prepared from the following raw materials in parts by weight:

[0148] 75-85 parts of silicone modified acrylic resin; 45 parts of silicone modified polyester resin; 11 parts of negative oxygen ion essence; 6 parts of ultrafine light calcium; 35 parts of solvent; 5 parts of activated carbon powder; 0.6 parts of curing agent; 0.6 parts of dispersant; 0.2 parts of defoaming agent; 0.2 parts of wetting agent; 0.2 parts of thickener; 0.1 parts of mildewproof agent; 0.2 parts of leveling agent; 1.4 parts of antibacterial agent; 0.58 parts of film-forming aid; 0.2 parts of anti-settling agent.

[0149] Among them, the solvent is diethylene glycol butyl ether; the curing agent is water-dispersible polyisocyanate; the dispersant is sodium polyacrylate; the defoaming agent is polysiloxane copolymer; the wetting agent is polyether modified siloxane; the thickener is a polyurethane thickener; the mildewproof agent is 361 mildewproof agent; the leveling agent is acrylic acid; the antibacterial agent is nanosilver colloidal solution; the film-forming aid is dipropylene glycol methyl ether; and the anti-settling agent is bentonite.

[0150] The preparation method of the negative oxygen ion ecological coating specifically comprises the following steps:

[0151] (1) mixing an organosilicon-modified acrylic resin and an organosilicon-modified polyester resin in a mixer, and controlling the mixing temperature at 50° C.;

[0152] (2) adding ultrafine light calcium, solvent, activated carbon powder, curing agent, dispersant, defoamer, wetting agent, thickener, mildewproof agent, leveling agent, antibacterial agent, film-forming aid, and anti-settling agent, and mixing and stirring in a high-speed stirrer at 1000 rpm;

[0153] (3) Finally, negative oxygen ion essence is added, and ultrasonic treatment is applied for 15 minutes, and then mixed and stirred in a high-speed mixer to obtain negative oxygen ion ecological paint.

[0154] The negative oxygen ion essence is prepared from the following raw materials in percentage by mass:

[0155] 18.5% of nano-tourmaline particles, 16.5% of ultrafine diatomaceous earth particles, 0.5% of dispersant, 0.5% of anionic surfactant, and the balance of plant extract.

[0156] The preparation steps of negative oxygen ion essence include:

[0157] Mix nano tourmaline particles, ultrafine diatomaceous earth particles, dispersant, anionic surfactant and plant extract, mix and stir in a high-speed blender, control the stirring speed at 1500rpm, and after the stirring is completed, the negative oxygen ion essence is obtained.

[0158] The method for preparing the plant extract specifically comprises the following steps:

[0159] (1) crushing and mixing ivy, mint, and aloe, freezing and crushing, pulverizing in a high-speed crusher, further grinding and refining in an ultrafine grinder, washing with 15° C. purified water, mixing and dispersing in a high-speed stirrer at 1500 rpm, removing the upper floating matter, standing at a constant temperature of 15° C. for 12 hours, filtering, and obtaining a filtrate and a filter residue;

[0160] (2) drying the filter residue at 60° C. for 3 h, and further grinding the powder obtained after drying, and passing it through a 500-mesh sieve to obtain a plant extract powder;

[0161] (3) The filtrate was concentrated to half of its original volume, and then a surfactant and the above-mentioned plant extract powder were added, and mixed and dispersed in a high-speed stirrer at 1200 rpm to obtain a plant extract solution.

[0162] Performance testing:

[0163] 1. Water vapor transmission resistance test and negative oxygen ion quantity test of coatings:

[0164] (1) The coating prepared in the specific implementation method is coated on a carrier, and then the carrier is placed in a sealed chamber filled with a mixture of heated saturated air and water vapor. The indoor temperature is generally maintained at 38°C. At 100% relative humidity, the slight temperature difference between the coating and the surrounding water vapor will cause water droplets to condense on the sample. The external conditions can be adjusted by changing the test time. The water droplets penetrate into the coating of the coating. The penetration speed is determined by the performance of the coating itself. Color changes, blistering, decreased adhesion, softening, embrittlement, etc. are detected, and the number of negative oxygen ions in the sealed chamber is also measured.

[0165] According to the above, a comparative example is set up: the coating prepared in Example 1 is coated on a carrier, and then the carrier is placed in an air-tight chamber filled with a mixture of heated saturated steam, and the indoor temperature is generally maintained at 38°C, and the number of negative oxygen ions in the sealed chamber is detected at different relative humidities;

[0166] Comparative Example 1: The humidity of the air in the sealed chamber is 95% relative humidity;

[0167] Comparative Example 2: The humidity of the air in the sealed chamber is 90% relative humidity;

[0168] Comparative Example 3: The humidity of the air in the sealed chamber is 85% relative humidity;

[0169] Comparative Example 4: The humidity of the air in the sealed chamber is 80% relative humidity;

[0170] Comparative Example 5: The humidity of the air in the sealed chamber is 75% relative humidity;

[0171] Comparative Example 6: The humidity of the air in the sealed chamber is 70% relative humidity;

[0172] Comparative Example 7: The humidity of the air in the sealed chamber is 65% relative humidity;

[0173] Comparative Example 8: The humidity of the air in the sealed chamber is 60% relative humidity;

[0174] Comparative Example 9: The humidity of the air in the sealed chamber is 55% relative humidity;

[0175] Comparative Example 10: The humidity of the air in the sealed chamber was 50% relative humidity.

[0176] Establish a control group: apply the existing commercially available negative oxygen ion coating on the carrier, and then put the carrier into an air-sealed chamber filled with a mixture of heated saturated steam. Generally, the indoor temperature is maintained at 38°C, and the number of negative oxygen ions in the sealed chamber is detected at different relative humidities;

[0177] Control group 1: The humidity of the air in the sealed chamber was 95% relative humidity;

[0178] Control group 2: The humidity of the air in the sealed chamber was 90% relative humidity;

[0179] Control group 3: the humidity of the air in the sealed chamber was 85% relative humidity;

[0180] Control group 4: the humidity of the air in the sealed chamber was 80% relative humidity;

[0181] Control group 5: the humidity of the air in the sealed chamber was 75% relative humidity;

[0182] Control group 6: the humidity of the air in the sealed chamber was 70% relative humidity;

[0183] Control group 7: the humidity of the air in the sealed chamber was 65% relative humidity; Control group 8: the humidity of the air in the sealed chamber was 60% relative humidity; Control group 9: the humidity of the air in the sealed chamber was 55% relative humidity; Control group 10: the humidity of the air in the sealed chamber was 50% relative humidity.

[0184] Table 1:

[0185]

[0186] Table 2:

[0187]

[0188]

[0189] Based on Table 1 and Table 2, we can conclude that:

[0190] (1) The coating prepared in this embodiment has good waterproof and mildew-proof properties, and the coating has a high continuous release of negative oxygen ions and a stable release;

[0191] (2) It can be concluded from the comparative examples that the relative humidity of the air has a direct impact on the release of negative oxygen ions from the coating. When the relative humidity of the air decreases, the continuous release of negative oxygen ions from the coating decreases. It can be concluded from the comparative examples and the control group that when the relative humidity of the air decreases, the rate of change in the amount of negative oxygen ions released by the coating prepared by the present invention is smaller.

[0192] 2. According to the standards of GB18582-2008 "Limits of Harmful Substances in Interior Wall Coatings for Interior Decoration and Decoration Materials" and JG / T24-2000 "Synthetic Resin Emulsion Sand Wall Architectural Coatings", the coating prepared in this embodiment was tested:

[0193] Table 3: Hazardous substance limit requirements:

[0194]

[0195] Table 4:

[0196]

[0197] Table 5:

[0198]

[0199] The negative oxygen ion ecological paint prepared in this embodiment is green and environmentally friendly. After testing, it all meets the requirements of the standards of GB18582-2008 "Limits of Harmful Substances in Interior Wall Paints for Interior Decoration and Decorative Materials" and "Synthetic Resin Emulsion Sand Wall Architectural Paint" JG / T24-2000.

[0200] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

[0201] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A negative oxygen ion ecological paint, characterized in that: The negative oxygen ion ecological paint is prepared from the following raw materials in parts by weight: 70-90 parts of silicone modified acrylic resin; 40-60 parts of silicone modified polyester resin; 10-15 portions of negative oxygen ion essence; 5-10 portions of ultrafine light calcium; 30-55 parts of solvent; 3-10 parts of activated carbon powder; Curing agent 0.5-1 part; Dispersant 0.5-1 part; Defoaming agent 0.1-0.5 parts; Wetting agent 0.1-0.5 parts; Thickener 0.1-0.5 parts; 0.1-0.3 parts of mildew inhibitor; Leveling agent 0.1-0.5 parts; 1-2.5 parts of antibacterial agent; Film-forming aid 0.4-0.9 parts; Anti-settling agent 0.1-0.5 parts.

2. The negative oxygen ion ecological paint according to claim 1, characterized in that: The negative oxygen ion ecological paint is prepared from the following raw materials in parts by weight: 75-85 parts of silicone modified acrylic resin; 45-55 parts of silicone modified polyester resin; Negative oxygen ion essence 11-13 parts; 6-8 portions of ultrafine light calcium; 35-50 parts of solvent; 5-7 parts of activated carbon powder; Curing agent 0.6-0.8 parts; Dispersant 0.6-0.8 parts; Defoaming agent 0.2-0.4 parts; Wetting agent 0.2-0.4 parts; Thickener 0.2-0.4 parts; 0.1-0.2 parts of mildew inhibitor; Leveling agent 0.2-0.4 parts; Antibacterial agent 1.4-2 parts; Film-forming aid 0.5-0.8 parts; Anti-settling agent 0.2-0.4 parts.

3. The negative oxygen ion ecological paint according to claim 1, characterized in that: The negative oxygen ion ecological paint is prepared from the following raw materials in parts by weight: 80 parts of silicone modified acrylic resin; 50 parts of silicone modified polyester resin; Negative oxygen ion essence 12 servings; 7 parts of ultra-fine light calcium; 42 parts of solvent; 6.5 parts of activated carbon powder; 0.7 parts of curing agent; Dispersant 0.7 parts; 0.3 parts of defoaming agent; Wetting agent 0.3 parts; Thickener 0.3 parts; 0.1-0.2 parts of mildew inhibitor; 0.3 parts of leveling agent; 1.7 parts of antibacterial agent; 0.7 parts of film-forming aid; 0.3 parts of anti-settling agent.

4. The negative oxygen ion ecological paint according to claim 1, characterized in that: The solvent diethylene glycol butyl ether; The curing agent is a water-dispersible polyisocyanate; The dispersant is SN-5040 or sodium salt of polycarboxylate or sodium polyacrylate or sodium lauryl sulfate; The defoamer is fatty acid amide or polysiloxane copolymer; The wetting agent is polyether modified siloxane; The thickener is a polyurethane thickener; The mildewcide is 361 mildewcide; The leveling agent is a fluorocarbon leveling agent or acrylic acid or MOK-2050; The antibacterial agent is a nano silver colloid solution; The film-forming aid is ester alcohol lauryl or dipropylene glycol methyl ether or tripropylene glycol butyl ether; The anti-settling agent is bentonite.

5. The method for preparing the negative oxygen ion ecological coating according to any one of claims 1 to 4, characterized in that: The preparation method specifically comprises the following steps: (1) mixing an organosilicon-modified acrylic resin and an organosilicon-modified polyester resin in a high-speed mixer, and controlling the mixing temperature at 45-50° C.; (2) adding ultrafine light calcium, solvent, activated carbon powder, curing agent, dispersant, defoamer, wetting agent, thickener, mildewproof agent, leveling agent, antibacterial agent, film-forming aid, and anti-settling agent, and mixing and stirring in a high-speed stirrer at 800-1000 rpm; (3) Finally, add the negative oxygen ion essence and apply ultrasonic treatment for 10-15 minutes, and then mix and stir in a high-speed mixer to obtain the negative oxygen ion ecological paint.

6. The method for preparing the negative oxygen ion ecological coating according to claim 5, characterized in that: The negative oxygen ion essence is prepared from the following raw materials in percentage by mass: 15-20% of nano-tourmaline particles, 15-20% of ultrafine diatomaceous earth particles, 0.1-1% of dispersant, 0.1-0.5% of anionic surfactant, and the balance of plant extract.

7. The method for preparing the negative oxygen ion ecological coating according to claim 6, characterized in that: The negative oxygen ion essence is prepared from the following raw materials in percentage by mass: 16.5% of nano-tourmaline particles, 18% of ultrafine diatomaceous earth particles, 0.4% of dispersant, 0.3% of anionic surfactant, and the balance of plant extract.

8. The method for preparing the negative oxygen ion ecological coating according to claim 7, characterized in that: The preparation steps of the negative oxygen ion essence are as follows: nano tourmaline particles, ultrafine diatomaceous earth particles, dispersant, anionic surfactant and plant extract are mixed, mixed and stirred in a high-speed blender, and the stirring speed is controlled at 1200-1500rpm. After the stirring is completed, the negative oxygen ion essence is obtained.

9. The method for preparing the negative oxygen ion ecological coating according to claim 8, characterized in that: The preparation method of the plant extract specifically comprises the following steps: (1) crushing and mixing ivy, mint, and aloe, freezing and crushing, pulverizing in a high-speed crusher, and further grinding in an ultrafine grinder, then washing with 10-15° C. purified water, mixing and dispersing in a high-speed stirrer at 1200-1500 rpm, removing the upper floating matter, standing at a constant temperature of 10-15° C. for 10-12 hours, and filtering to obtain a filtrate and a filter residue; (2) drying the filter residue at 55-60° C. for 2-3 hours, and further grinding the powder obtained after drying, and passing it through a 500-mesh sieve to obtain a plant extract powder; (3) The filtrate is concentrated to half of its original volume, and then a surfactant and the above-mentioned plant extract powder are added, mixed and dispersed in a high-speed stirrer at 1000-1200 rpm, and the plant extract is obtained by discharging.