Corrosion-resistant coating
By using corrosion-resistant coatings composed of water-based polyester resins, epoxy resins, etc., combined with acrylic emulsions and other components, the problem of poor performance of existing coatings in harsh environments is solved, and effective protection and long-lasting use is achieved under acid rain. Reduced costs.
Patent Information
- Application Number
- CN202410916685.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing environmentally friendly anticorrosion coatings are difficult to meet user needs in harsh corrosion environments. The paint has poor peeling and anticorrosion performance, making it difficult to maintain corrosion resistance in high-temperature environments.
Corrosion-resistant coatings composed of water-based polyester resin, epoxy resin, phenolic resin, amino resin, etc., combined with acrylic emulsion, propylene glycol butyl ether, zinc phosphate and other components, high-solid content organic components and environmentally friendly solvents are used to form high performance. Coating, suitable for protection of various metal surfaces.
Maintain good corrosion resistance in harsh environments such as acid rain, extend service life, reduce costs, avoid frequent brushing, and provide effective protection.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of environmentally friendly anti-corrosion coatings, and in particular relates to a corrosion-resistant coating. Background Art
[0002] In the prior art, many environmental protection equipment are exposed to wind and rain for a long time, and the anti-corrosion performance of the equipment surface is required to be extremely high; there are many means to prevent the corrosion of metal materials, such as the use of corrosion-resistant metal materials, cathodic protection, corrosion inhibitors and metal protective coatings. Practice has proved that among the above metal anti-corrosion methods, the use of environmentally friendly anti-corrosion coatings to protect easily corroded metal materials is the most economical, effective and widely used anti-corrosion method. Conventional anti-corrosion coatings play an anti-corrosion role on metals under general conditions, thereby increasing the service life of non-ferrous metals; however, conventional anti-corrosion coatings cannot be used in relatively harsh corrosive environments, and it is difficult to meet the user's demand for the anti-corrosion ability of coatings. After a period of use, the surface of environmental protection equipment under the anti-corrosion coating will fall off and the anti-corrosion performance is poor.
[0003] Anti-corrosion coatings are mainly applied on the surface of objects to form a thin film or to play a protective or decorative role. For example, the existing patent document CN108219607 A discloses an anti-corrosion water-based coating. The obtained water-based coating has good corrosion resistance and can be applied to coatings in various industries. However, the prior art still has the problem that after the coating is applied to the surface of an object, as the environment changes, the corrosion resistance and high temperature resistance are poor. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a corrosion-resistant coating in view of the deficiencies of the background technology.
[0005] The present invention adopts the following technical solutions to solve the above technical problems:
[0006] A corrosion-resistant coating comprises the following ingredients in parts by weight: 20-35 parts of water-based polyester resin, 10-15 parts of epoxy resin, 5-15 parts of phenolic resin, 1-2 parts of amino resin, 30-50 parts of acrylic emulsion, 20-30 parts of propylene glycol butyl ether, 12-20 parts of dioctyl phthalate, 6-10 parts of polytetrafluoroethylene fiber, 3-6 parts of zinc phosphate, 3-6 parts of calcium carbonate, 2-4 parts of graphite powder, 3-6 parts of silicon dioxide, 5-10 parts of sodium fluorosilicate, 3-6 parts of 4-propyleneoxy-2-hydroxybenzophenone, 2-5 parts of silane coupling agent, 10-20 parts of sodium carboxymethyl cellulose, 8-20 parts of curing agent and 10-50 parts of solvent.
[0007] As a further preferred embodiment of the corrosion-resistant coating of the present invention, the epoxy resin is selected from at least one of bisphenol A epoxy resin, bisphenol F epoxy resin, polyphenol glycidyl ether epoxy resin, aliphatic glycidyl ether epoxy resin, glycidyl ester epoxy resin and heterocyclic epoxy resin.
[0008] As a further preferred embodiment of the corrosion-resistant coating of the present invention, the water-based polyester resin is a mixture of one or more of neopentyl glycol, adipic acid, phthalic acid, isophthalic anhydride, trimellitic anhydride, a catalyst, an antioxidant, a neutralizer and water.
[0009] As a further preferred embodiment of the corrosion-resistant coating of the present invention, the phenolic resin is mainly made of 100-265 parts of resin, 1-5 parts of aniline, 1-5 parts of ammonium acetate, 1-5 parts of polyaniline, 10-30 parts of metal magnesium, 10-18 parts of metal titanium, 3-7 parts of silicon oxide, 3-9 parts of magnesium oxide, 4-15 parts of cassia seeds, 8-5 parts of star anise, 15-5 parts of vaseline, 19-3 parts of glass fiber, 18-15 parts of methacrylic acid, 3-5 parts of cotton fiber, 1-8 parts of propylene, 3-13 parts of diamond powder, 3-18 parts of diatomaceous earth, 3-21 parts of norfloxacin, 3-19 parts of shell powder, 2-6 parts of feldspar powder and 1-9 parts of calcium bicarbonate.
[0010] As a further preferred embodiment of the corrosion-resistant coating of the present invention, the amino resin is prepared from melamine and formaldehyde solution as main raw materials, anion powder, nano silver ions, pH regulator and curing agent are added, and the mixture is synthesized at a temperature of 70-85°C.
[0011] As a further preferred embodiment of the corrosion-resistant coating of the present invention, the silane coupling agent is KH-560.
[0012] As a further preferred embodiment of the corrosion-resistant coating of the present invention, the acrylic emulsion is composed of pure acrylic emulsion and silicone acrylic emulsion in a weight ratio of 1:2.
[0013] As a further preferred embodiment of the corrosion-resistant coating of the present invention, the curing agent is one or a mixture of two or more of aliphatic amines, aromatic amines, alicyclic amines or amine-modified curing agents.
[0014] As a further preferred embodiment of the corrosion-resistant coating of the present invention, the solvent is a mixture of one of toluene, xylene, and styrene and one of n-butanol, isobutanol, tert-butanol, butanone, and cyclohexanone or two or more thereof.
[0015] Compared with the prior art, the present invention adopts the above technical solution and has the following technical effects:
[0016] 1. A corrosion-resistant coating of the present invention uses a low molecular weight polymer as a base resin to obtain a coating of an organic component with a high solid content, uses an environmentally friendly solvent as a diluent, has a simple preparation process, and is suitable for corrosion protection of various metal surfaces;
[0017] 2. The coating prepared by the invention has good corrosion resistance under the joint action of various raw materials, and can still maintain good performance under the long-term erosion of acid rain, so that outdoor materials can be effectively protected and prevented from being damaged by acid rain. The coating prepared by the invention is used for protection, with good protection effect and long service life, and no need to frequently repaint, which is more convenient and effectively reduces costs;
[0018] 3. This phenolic resin has good physical and chemical properties, a very wide range of applications, and is light in weight, with a simple formula and easy-to-obtain raw materials. DETAILED DESCRIPTION
[0019] The technical solution of the present invention is further described in detail below:
[0020] In order to make the above-mentioned purpose, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.
[0021] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0022] A corrosion-resistant coating comprises the following ingredients in parts by weight: 20-35 parts of water-based polyester resin, 10-15 parts of epoxy resin, 5-15 parts of phenolic resin, 1-2 parts of amino resin, 30-50 parts of acrylic emulsion, 20-30 parts of propylene glycol butyl ether, 12-20 parts of dioctyl phthalate, 6-10 parts of polytetrafluoroethylene fiber, 3-6 parts of zinc phosphate, 3-6 parts of calcium carbonate, 2-4 parts of graphite powder, 3-6 parts of silicon dioxide, 5-10 parts of sodium fluorosilicate, 3-6 parts of 4-propyleneoxy-2-hydroxybenzophenone, 2-5 parts of silane coupling agent, 10-20 parts of sodium carboxymethyl cellulose, 8-20 parts of curing agent and 10-50 parts of solvent.
[0023] The epoxy resin is selected from at least one of bisphenol A epoxy resin, bisphenol F epoxy resin, polyphenol glycidyl ether epoxy resin, aliphatic glycidyl ether epoxy resin, glycidyl ester epoxy resin and heterocyclic epoxy resin.
[0024] The waterborne polyester resin is one or a mixture of two or more of neopentyl glycol, adipic acid, phthalic acid, isophthalic anhydride, trimellitic anhydride, a catalyst, an antioxidant, a neutralizer and water.
[0025] The phenolic resin is mainly made of 100-265 parts of resin, 1-5 parts of aniline, 1-5 parts of ammonium acetate, 1-5 parts of polyaniline, 10-30 parts of metal magnesium, 10-18 parts of metal titanium, 3-7 parts of silicon oxide, 3-9 parts of magnesium oxide, 4-15 parts of cassia seeds, 8-5 parts of star anise, 15-5 parts of vaseline, 19-3 parts of glass fiber, 18-15 parts of methacrylic acid, 3-5 parts of cotton fiber, 1-8 parts of propylene, 3-13 parts of diamond powder, 3-18 parts of diatomaceous earth, 3-21 parts of norfloxacin, 3-19 parts of shell powder, 2-6 parts of feldspar powder and 1-9 parts of calcium bicarbonate.
[0026] The amino resin is prepared by using melamine and formaldehyde solution as main raw materials, adding negative ion powder, nano silver ions, a pH regulator and a curing agent, and is synthesized at a temperature of 70-85°C.
[0027] 1. Select melamine raw materials with a purity of ≥99.8%;
[0028] 2. Select 37% formaldehyde solution;
[0029] 3. Curing agent: hexamethylenetetramine;
[0030] 4. PH regulator: triethanolamine;
[0031] 5. Water-soluble negative ion powder, particle size ≤ 6μm;
[0032] 6. Nano silver ions, particle size is 1000-2000nm, heat resistance temperature is 300℃;
[0033] 7. Synthesize in appropriate proportions at 70-85°C.
[0034] The silane coupling agent is KH-560.
[0035] The acrylic emulsion is composed of pure acrylic emulsion and silicone acrylic emulsion in a weight ratio of 1:2.
[0036] The curing agent is one or a mixture of two or more of aliphatic amine, aromatic amine, alicyclic amine or amine-modified curing agent.
[0037] The solvent is one of toluene, xylene and styrene and one of n-butanol, isobutanol, tert-butanol, butanone and cyclohexanone or a mixture of two or more thereof.
[0038] The present invention discloses a corrosion-resistant coating. The present invention uses a low molecular weight polymer as a base resin to obtain a coating with a high solid content of organic components, uses an environmentally friendly solvent as a diluent, has a simple preparation process, and is suitable for corrosion protection of various metal surfaces.
[0039] The coating prepared by the invention has good corrosion resistance under the combined effect of various raw materials, and can still maintain good performance under long-term erosion by acid rain, so that outdoor materials can be effectively protected to avoid damage caused by acid rain to outdoor materials. The coating prepared by the invention is used for protection, and has good protection effect and long service life. There is no need to frequently repaint the coating, which is more convenient and effectively reduces costs.
[0040] The phenolic resin has good physical and chemical properties, a very wide range of applications, and is light in weight, has a simple formula and easily available raw materials.
[0041] A preparation method based on corrosion-resistant coating, specifically comprising the following steps;
[0042] Step 1, heating a water-based polyester resin, an epoxy resin, a phenolic resin, an amino resin, an acrylic emulsion, and a solvent to 80-100° C., stirring while heating, adding propylene glycol butyl ether and dioctyl phthalate after heating, stirring at a speed of 300-500 r / min for 20-30 min, cooling, and obtaining a mixed emulsion 1;
[0043] Step 2, adding zinc phosphate, calcium carbonate, graphite powder, silicon dioxide, sodium fluorosilicate, 4-propyleneoxy-2-hydroxybenzophenone, silane coupling agent carboxyl, sodium methyl cellulose, a curing agent, and a solvent to the mixed emulsion obtained in step 1), and stirring at a speed of 800-1000 r / min for 10-20 min to obtain a mixed emulsion 2;
[0044] Step 3: Add polytetrafluoroethylene fiber to the mixed emulsion 2 obtained in step 2), disperse it in an ultrasonic environment with a frequency of 20-30KHz for 15-25 minutes, discharge it, and let it stand for 1-2 hours to obtain a corrosion-resistant coating;
[0045] Step 4, placing the barrel to be filled under the processing device, and quickly adding the corrosion-resistant coating into the barrel through the processing device;
[0046] Step 5, sealing the storage barrel to obtain barreled corrosion-resistant coating.
[0047] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A corrosion-resistant coating, characterized in that: The invention comprises the following ingredients in parts by weight: 20-35 parts of water-based polyester resin, 10-15 parts of epoxy resin, 5-15 parts of phenolic resin, 1-2 parts of amino resin, 30-50 parts of acrylic emulsion, 20-30 parts of propylene glycol butyl ether, 12-20 parts of dioctyl phthalate, 6-10 parts of polytetrafluoroethylene fiber, 3-6 parts of zinc phosphate, 3-6 parts of calcium carbonate, 2-4 parts of graphite powder, 3-6 parts of silicon dioxide, 5-10 parts of sodium fluorosilicate, 3-6 parts of 4-propyleneoxy-2-hydroxybenzophenone, 2-5 parts of silane coupling agent, 10-20 parts of sodium carboxymethyl cellulose, 8-20 parts of curing agent and 10-50 parts of solvent.
2. A corrosion-resistant coating according to claim 1, characterized in that: The epoxy resin is selected from at least one of bisphenol A epoxy resin, bisphenol F epoxy resin, polyphenol glycidyl ether epoxy resin, aliphatic glycidyl ether epoxy resin, glycidyl ester epoxy resin and heterocyclic epoxy resin.
3. A corrosion-resistant coating according to claim 1, characterized in that: The waterborne polyester resin is one or a mixture of two or more of neopentyl glycol, adipic acid, phthalic acid, isophthalic anhydride, trimellitic anhydride, a catalyst, an antioxidant, a neutralizer and water.
4. The corrosion-resistant coating according to claim 1, characterized in that: The phenolic resin is mainly made of 100-265 parts of resin, 1-5 parts of aniline, 1-5 parts of ammonium acetate, 1-5 parts of polyaniline, 10-30 parts of metal magnesium, 10-18 parts of metal titanium, 3-7 parts of silicon oxide, 3-9 parts of magnesium oxide, 4-15 parts of cassia seeds, 8-5 parts of star anise, 15-5 parts of vaseline, 19-3 parts of glass fiber, 18-15 parts of methacrylic acid, 3-5 parts of cotton fiber, 1-8 parts of propylene, 3-13 parts of diamond powder, 3-18 parts of diatomaceous earth, 3-21 parts of norfloxacin, 3-19 parts of shell powder, 2-6 parts of feldspar powder and 1-9 parts of calcium bicarbonate.
5. The corrosion-resistant coating according to claim 1, characterized in that: The amino resin is prepared by using melamine and formaldehyde solution as main raw materials, adding negative ion powder, nano silver ions, a pH regulator and a curing agent, and is synthesized at a temperature of 70-85°C.
6. The corrosion-resistant coating according to claim 1, characterized in that: The silane coupling agent is KH-560.
7. The corrosion-resistant coating according to claim 1, characterized in that: The acrylic emulsion is composed of pure acrylic emulsion and silicone acrylic emulsion in a weight ratio of 1:
2.
8. The corrosion-resistant coating according to claim 1, characterized in that: The curing agent is one or a mixture of two or more of aliphatic amine, aromatic amine, alicyclic amine or amine-modified curing agent.
9. The corrosion-resistant coating according to claim 1, characterized in that: The solvent is one of toluene, xylene and styrene and one of n-butanol, isobutanol, tert-butanol, butanone and cyclohexanone or a mixture of two or more thereof.
Citation Information
Patent Citations
Anti-corrosion water-based paint
CN108219607A