Nano silicon modified resin coating and preparation method thereof
Through the synergistic effect of nano-silicon modified alkyd resin and composite drying agent, the surface uneven problem caused by the drying speed of alkyd resin coating is solved, and the effect of high gloss and rapid drying is achieved.
Patent Information
- Application Number
- CN202411067210.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The drying speed of alkyd resin coatings is too fast, resulting in uneven and rough surface of the coating film, affecting gloss.
The gloss and drying speed of the coating film are improved by ultrasonic mixing of organic nanosilicon and alkyd resin and a specific drying agent.
The synergistic effect of nano-silicon modified alkyd resin and composite drying agent improves the gloss and drying speed of the paint, ensures smooth surface of the coating, and improves the leveling speed and gloss.
Smart Images

Figure CN118931337A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of alkyd resin coatings, and in particular relates to a nano-silicon modified resin coating and a preparation method thereof. Background Art
[0002] Alkyd resin is a synthetic resin with broad application prospects, mainly composed of polyols, phthalic anhydride and fatty acids or oils through condensation polymerization. It has good gloss, toughness and adhesion, as well as excellent wear resistance, weather resistance and insulation properties. In order to speed up the drying and film formation speed and shorten the construction period, coatings made with alkyd resin as the base usually use driers. Driers play a role in accelerating curing and improving the quality of the coating film, significantly improving the hardness and durability of the coating.
[0003] However, experiments have found that when the coating dries too quickly, the solvent or dispersion medium evaporates too quickly, so that the coating does not have enough time to level, and eventually forms a poor surface state, which will cause the coating surface to become uneven and rough, thereby affecting the gloss of the coating. Summary of the invention
[0004] In order to solve the problems existing in the background technology, the present invention provides a nano-silicon modified resin coating and a preparation method thereof, which can accelerate the drying speed of the coating film and improve the glossiness of the coating film.
[0005] In order to achieve the above-mentioned purpose, in a first aspect, the present invention provides a nano-silicon modified resin coating, which comprises the following raw material components in parts by weight: 100 parts of nano-silicon modified alkyd resin, 1-1.4 parts of composite drying agent, 25-30 parts of composite powder filler, 40-45 parts of xylene, 0.6-1 part of dispersant, 0.4-0.7 part of defoaming agent and 0.3-0.5 part of anti-skinning agent; the nano-silicon modified alkyd resin is prepared by ultrasonic mixing of organic nano-silicon and alkyd resin in a mass ratio of 1:40-45.
[0006] Furthermore, the specific preparation method of the nano-silicon modified alkyd resin is as follows:
[0007] A1. Add organic nano-silicon into alkyd resin, stir at a speed of 100-120r / min for 8-10min to obtain a mixture;
[0008] A2. The mixture obtained in A1 is subjected to 35-40KHz low-frequency ultrasonic treatment for 3-4 hours to obtain nano-silicon modified alkyd resin.
[0009] Further, the preparation method of organic nano silicon:
[0010] A11, weigh 25g of nano-silicon powder, disperse it in 750mL of distilled water, stir and heat to 80°C, add 22-25g of 30% by mass hexadecyltrimethylammonium bromide aqueous solution, heat to 90°C, keep constant temperature for 2h, and treat with ultrasonic vibration for 0.5h to obtain the product;
[0011] A12. Filter the product obtained in A11, wash it with distilled water, let it stand for 12 hours, then filter it again and wash it again. Repeat this process several times until the product is identified as Br free using AgNO3 solution. - Then, put it into a drying oven and dry it at 138-142°C to constant weight to obtain organic nano-silicon.
[0012] Furthermore, the preparation method of the composite drying agent is as follows: 8% cobalt isooctanoate, 8% manganese isooctanoate, 12% zirconium isooctanoate, 5% calcium isooctanoate, 9% zinc isooctanoate and bipyridine are mixed in a mass ratio of 9:5:(5-6):2:1:0.1 and mixed evenly to obtain the composite drying agent.
[0013] Furthermore, the preparation method of the composite powder filler is as follows:
[0014] B1. Mix heavy calcium powder and light calcium powder in a mass ratio of (2-3):1 to obtain a mixed powder;
[0015] B2. By weight, 35 parts of the mixed powder obtained from B1 are fed into an activation batching machine, the speed is set to 600-800r / min, the temperature is set to 70-80°C, and then 0.2-0.3 parts of stearate and 0.2-0.3 parts of hydrogen-containing silicone oil are added, the temperature is maintained and stirred for 20-25 minutes to obtain a composite powder filler.
[0016] Furthermore, the dispersant includes BYK-109 dispersant or BYK-164 dispersant.
[0017] Furthermore, the defoaming agent is EFKA-2526 defoaming agent.
[0018] Furthermore, the anti-skinning agent is Milliken BNK-DSF1010 anti-skinning agent.
[0019] In a second aspect, the present invention provides a method for preparing the above-mentioned nano-silicon modified resin coating, comprising the following steps:
[0020] S1. Put the nano-silicon modified alkyd resin into a disperser, control the stirring speed at 450-500r / min, add a composite drier, a composite powder filler, xylene, a dispersant, a defoamer and an anti-skinning agent, and continue stirring for 15-25min to obtain a primary material;
[0021] S2. Grind the primary material obtained in S1 to a fineness of no more than 25 μm to obtain a nano-silicon modified resin coating.
[0022] This application has the following beneficial effects:
[0023] 1. The present invention adopts nano-silicon modified alkyd resin and composite drying agent. Experimental verification shows that the addition of nano-silicon modified alkyd resin can improve the gloss of the obtained coating; the addition of composite drying agent can accelerate the actual drying speed of the coating film and also improve the gloss of the obtained coating; and there is a synergistic effect between the two, which can synergistically improve the gloss of the obtained coating.
[0024] 2. In the preparation of the nano-silicon modified alkyd resin of the present invention, the mixing process allows the organic nano-silicon to be uniformly dispersed in the alkyd resin as a filler. This dispersibility is due to the good dispersibility of the organic nano-silicon and the wettability of the alkyd resin. The well-dispersed nano-silicon can better reduce the viscosity of the alkyd resin, thereby improving its fluidity. In addition, due to the small particle size of the organic nano-silicon, it can fill the tiny defects in the alkyd resin coating, thereby forming a smoother surface on a macro scale, which is beneficial to increase the leveling speed and enhance the glossiness. The addition of organic nano-silicon can also change the surface tension of the alkyd resin, which helps the coating to reach a balanced state more quickly during the curing process and dry faster.
[0025] 3. In the preparation of the composite drying agent of the present invention, 8% cobalt isooctanoate is conducive to rapid surface drying, 8% manganese isooctanoate is conducive to bottom drying and actual drying, 5% calcium isooctanoate and 9% zinc isooctanoate are used as auxiliary ingredients to maintain the balance between surface drying and actual drying, and 12% zirconium isooctanoate is used as a coordination polymerization drying agent. Zirconium can complex with hydroxyl groups and other polar groups (epoxy groups) in alkyd resin to generate a coordination complex with a larger molecular weight, which becomes a component of the coating film, and cooperates with cobalt and manganese driers to effectively improve the drying performance, accelerate the drying speed of the coating film, and improve the gloss of the coating film. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 , a comparative trend chart of the actual drying time test data of the resin coating brush plate coating films obtained in Examples 1-7 of the present invention and Comparative Examples 1-5;
[0027] Figure 2 , a comparative trend chart of gloss test data of resin coatings obtained from Examples 1-7 of the present invention and Comparative Examples 1-5. DETAILED DESCRIPTION
[0028] The present application is further described in detail below in conjunction with embodiments.
[0029] Unless otherwise specified, the raw materials used in the examples and comparative examples of the present application are all commercially available.
[0030] Example 1: (1) Preparation of organic nano-silicon, the preparation method is as follows:
[0031] A11. Weigh 25 g of nano-silicon powder, disperse it into 750 mL of distilled water, stir and heat to 80° C., add dropwise 23 g of 30% by mass hexadecyltrimethylammonium bromide aqueous solution, heat to 90° C., keep constant temperature for 2 h, and treat with ultrasonic vibration for 0.5 h to obtain the product.
[0032] A12. Filter the product obtained in A11, wash it with distilled water, let it stand for 12 hours, then filter it again and wash it again. Repeat this process several times until the product is identified as Br free using AgNO3 solution. - Then, the mixture was placed in a drying oven and dried at 140°C to constant weight to obtain organic nano-silicon.
[0033] Among them, nano silicon powder (Brofos-Si-30) with a spherical microscopic morphology and a purity of ≥99.9% was purchased from Bohuasi Nanotechnology (Ningbo) Co., Ltd. Hexadecyltrimethylammonium bromide (content 99%) was purchased from Hubei Kewode Chemical Co., Ltd.
[0034] (2) Preparation of nano-silicon modified alkyd resin, the specific preparation method is as follows:
[0035] A1. Add organic nano-silicon into alkyd resin, the mass ratio of organic nano-silicon to alkyd resin is 1:42, the rotation speed is 110r / min, and the mixture is stirred at a constant speed for 9 minutes to obtain a mixture.
[0036] A2. The mixture obtained in A1 was subjected to 38KHz low-frequency ultrasonic treatment for 3.5 hours to obtain nano-silicon modified alkyd resin.
[0037] Among them, alkyd resin (HD-389) is an oily alkyd resin purchased from Hongda Chemical Co., Ltd., Fengqiu County, Henan Province.
[0038] (3) Prepare a composite drier as follows: 8% cobalt 2-octanoate, 8% manganese 2-octanoate, 12% zirconium 2-octanoate, 5% calcium 2-octanoate, 9% zinc 2-octanoate and bipyridine are mixed in a mass ratio of 9:5:5.5:2:1:0.1, and mix well to obtain the drier. 8% cobalt 2-octanoate, 8% manganese 2-octanoate, 12% zirconium 2-octanoate, 5% calcium 2-octanoate and 9% zinc 2-octanoate are all mass fractions, and the solvent is xylene.
[0039] The relevant properties and parameters of each raw material component are listed in Table 1 below.
[0040] Table 1. Performance and parameters of each raw material component of the composite catalyst
[0041] name Appearance Metal content (%) Solution stability Cobalt 2-ethylhexanoate Purple liquid 8±0.2 Transparent without precipitates Manganese 2-ethylhexanoate Brown red liquid 8±0.2 Transparent without precipitates Zirconium 2-ethylhexanoate Light yellow liquid 12±0.2 Transparent without precipitates Calcium 2-ethylhexanoate Light yellow liquid 5±0.2 Transparent without precipitates Zinc 2-ethylhexanoate Yellow liquid 9±0.2 Transparent without precipitates
[0042] (4) The preparation method of the composite powder filler is as follows:
[0043] B1. Mix heavy calcium powder and light calcium powder in a mass ratio of 2:1 to obtain a mixed powder.
[0044] B2. By weight, 35 parts of the mixed powder obtained from B1 were fed into an activation batching machine, the speed was set to 700 r / min, the temperature was set to 75°C, and then 0.3 parts of stearate and 0.3 parts of hydrogen-containing silicone oil were added. The temperature was maintained and stirred for 23 minutes to obtain a composite powder filler.
[0045] Among them, heavy calcium powder (600 mesh) was purchased from Guangxi Hezhou Huaxiang New Materials Co., Ltd.; light calcium powder (1250 mesh) was purchased from Lingshou County Zhan Da Mineral Products Co., Ltd.
[0046] (5) Preparing a nano-silicon modified resin coating, the preparation method comprises the following steps:
[0047] S1. Put 100 parts of nano-silicon modified alkyd resin into a disperser by weight, control the stirring speed at 480r / min, add 1.2 parts of composite drier, 27 parts of composite powder filler, 44 parts of xylene, 0.7 parts of dispersant, 0.5 parts of defoamer and 0.4 parts of anti-skinning agent, and continue stirring for 20 minutes to obtain a primary material.
[0048] S2. Grind the primary material obtained in S1 to a fineness of no more than 25 μm (scraper) to obtain a nano-silicon modified resin coating.
[0049] The dispersant is BYK-109 dispersant, the defoamer is EFKA-2526 defoamer, and the anti-skinning agent is Milliken BNK-DSF1010 anti-skinning agent.
[0050] Example 2: The difference between this example and Example 1 is that organic nano-silicon is prepared by the following method:
[0051] A11. Weigh 25 g of nano-silicon powder, disperse it in 750 mL of distilled water, stir and heat to 80° C., add dropwise 22 g of 30% by mass hexadecyltrimethylammonium bromide aqueous solution, heat to 90° C., keep constant temperature for 2 h, and treat with ultrasonic vibration for 0.5 h to obtain the product.
[0052] A12. Filter the product obtained in A11, wash it with distilled water, let it stand for 12 hours, then filter it again and wash it again. Repeat this process several times until the product is identified as Br free using AgNO3 solution. - Then, the mixture was placed in a drying oven and dried at 138°C to constant weight to obtain organic nano-silicon.
[0053] Preparation of nano-silicon modified alkyd resin, the specific preparation method is as follows:
[0054] A1. Add organic nano-silicon into alkyd resin, the mass ratio of organic nano-silicon to alkyd resin is 1:40, the rotation speed is 100r / min, and the mixture is stirred at a constant speed for 8 minutes to obtain a mixture.
[0055] A2. The mixture obtained in A1 was subjected to 35KHz low-frequency ultrasonic treatment for 3 hours to obtain nano-silicon modified alkyd resin.
[0056] Example 3: The difference between this example and Example 1 is that organic nano-silicon is prepared by the following method:
[0057] A11. Weigh 25 g of nano-silicon powder, disperse it into 750 mL of distilled water, stir and heat to 80° C., add dropwise 25 g of 30% by mass hexadecyltrimethylammonium bromide aqueous solution, heat to 90° C., keep constant temperature for 2 h, and treat with ultrasonic vibration for 0.5 h to obtain the product.
[0058] A12. Filter the product obtained in A11, wash it with distilled water, let it stand for 12 hours, then filter it again and wash it again. Repeat this process several times until the product is identified as Br free using AgNO3 solution. - Then, the mixture was placed in a drying oven and dried at 142°C to constant weight to obtain organic nano-silicon.
[0059] Preparation of nano-silicon modified alkyd resin, the specific preparation method is as follows:
[0060] A1. Add organic nano-silicon into alkyd resin, the mass ratio of organic nano-silicon to alkyd resin is 1:45, and stir at a speed of 120r / min for 10min to obtain a mixture.
[0061] A2. The mixture obtained in A1 was subjected to 40KHz low-frequency ultrasonic treatment for 4 hours to obtain nano-silicon modified alkyd resin.
[0062] Example 4: The difference between this example and Example 1 is that a composite drying agent is prepared by mixing 8% cobalt isooctanoate, 8% manganese isooctanoate, 12% zirconium isooctanoate, 5% calcium isooctanoate, 9% zinc isooctanoate and bipyridine in a mass ratio of 9:5:5:2:1:0.1 and mixing well.
[0063] Example 5: The difference between this example and Example 1 is that a composite drying agent is prepared by mixing 8% cobalt isooctanoate, 8% manganese isooctanoate, 12% zirconium isooctanoate, 5% calcium isooctanoate, 9% zinc isooctanoate and bipyridine in a mass ratio of 9:5:6:2:1:0.1 and mixing well.
[0064] Embodiment 6: The difference between this embodiment and embodiment 1 is that: a nano-silicon modified resin coating is prepared, and the preparation method comprises the following steps:
[0065] S1. Put 100 parts of nano-silicon modified alkyd resin into a disperser by weight, control the stirring speed at 450r / min, add 1 part of composite drying agent, 25 parts of composite powder filler, 40 parts of xylene, 0.6 part of dispersant, 0.4 part of defoamer and 0.3 part of anti-skinning agent, and continue stirring for 15 minutes to obtain a primary material.
[0066] S2. Grind the primary material obtained in S1 to a fineness of no more than 25 μm to obtain a nano-silicon modified resin coating.
[0067] Embodiment 7: The difference between this embodiment and embodiment 1 is that: the nano-silicon modified resin coating is prepared, and the preparation method comprises the following steps:
[0068] S1. Put 100 parts of nano-silicon modified alkyd resin into a disperser by weight, control the stirring speed at 500r / min, add 1.4 parts of composite drying agent, 30 parts of composite powder filler, 45 parts of xylene, 1 part of dispersant, 0.7 parts of defoaming agent and 0.5 parts of anti-skinning agent, and continue stirring for 25 minutes to obtain a primary material.
[0069] S2. Grind the primary material obtained in S1 to a fineness of no more than 25 μm to obtain a nano-silicon modified resin coating.
[0070] Comparative Example 1: The difference between this comparative example and Example 1 is that the organic nano-silicon is replaced by nano-silicon powder.
[0071] Specifically, the nano-silicon modified alkyd resin is prepared, and the specific preparation method is as follows:
[0072] A1. Add nano-silicon powder into alkyd resin, the mass ratio of nano-silicon powder to alkyd resin is 1:42, the rotation speed is 110r / min, and the mixture is stirred at a constant speed for 9 minutes to obtain a mixture.
[0073] A2. The mixture obtained in A1 was subjected to 38KHz low-frequency ultrasonic treatment for 3.5 hours to obtain nano-silicon modified alkyd resin.
[0074] Comparative Example 2: The difference between this comparative example and Example 1 is that the nano-silicon modified alkyd resin is replaced by alkyd resin.
[0075] Specifically, the resin coating is prepared, and the preparation method comprises the following steps:
[0076] S1. Put 100 parts of alkyd resin into a disperser by weight, control the stirring speed at 480r / min, add 1.2 parts of composite drier, 27 parts of composite powder filler, 44 parts of xylene, 0.7 parts of dispersant, 0.5 parts of defoamer and 0.4 parts of anti-skinning agent, and continue stirring for 20 minutes to obtain a primary material.
[0077] S2. Grind the primary material obtained in S1 to a fineness of no more than 25 μm (scraper) to obtain a resin coating.
[0078] Comparative Example 3: The difference between this comparative example and Example 1 is that 12% of zirconium isooctanoate is deleted in the preparation of the composite drying agent.
[0079] Specifically, the composite drying agent is prepared as follows: 8% cobalt isooctanoate, 8% manganese isooctanoate, 5% calcium isooctanoate, 9% zinc isooctanoate and bipyridine are mixed in a mass ratio of 9:5:2:1:0.1 and mixed evenly to obtain the composite drying agent.
[0080] Comparative Example 4: The difference between this comparative example and Example 1 is that in the preparation of the composite drying agent, 12% of zirconium isooctanoate is replaced by 8% of manganese isooctanoate.
[0081] Specifically, the composite drying agent is prepared as follows: 8% cobalt isooctanoate, 8% manganese isooctanoate, 5% calcium isooctanoate, 9% zinc isooctanoate and bipyridine are mixed in a mass ratio of 9:10.5:2:1:0.1, and the mixture is uniformly mixed to obtain the composite drying agent.
[0082] Comparative Example 5: The difference between this comparative example and Example 1 is that the nano-silicon modified alkyd resin is replaced by alkyd resin, and 12% of zirconium isooctanoate is deleted in the preparation of the composite drying agent.
[0083] Specifically, the composite drying agent is prepared as follows: 8% cobalt isooctanoate, 8% manganese isooctanoate, 5% calcium isooctanoate, 9% zinc isooctanoate and bipyridine are mixed in a mass ratio of 9:5:2:1:0.1 and mixed evenly to obtain the composite drying agent.
[0084] The resin coating is prepared, and the preparation method comprises the following steps:
[0085] S1. Put 100 parts of alkyd resin into a disperser by weight, control the stirring speed at 480r / min, add 1.2 parts of composite drier, 27 parts of composite powder filler, 44 parts of xylene, 0.7 parts of dispersant, 0.5 parts of defoamer and 0.4 parts of anti-skinning agent, and continue stirring for 20 minutes to obtain a primary material.
[0086] S2. Grind the primary material obtained in S1 to a fineness of no more than 25 μm (scraper) to obtain a resin coating.
[0087] Test example: Test object: Resin coatings were prepared according to Examples 1-7 and Comparative Examples 1-5.
[0088] Test items: constant temperature and humidity drying; glossiness.
[0089] Test basis: constant temperature and humidity (35℃, 55%), actual drying time - cotton ball pressing method;
[0090] Gloss - GB / T 9754.
[0091] Test results: See Table 2.
[0092] Table 2. Test data of the experimental example
[0093] Constant temperature and humidity actual drying / h Glossiness / 60° angle, % Example 1 10.73 93.6 Example 2 10.65 93.2 Example 3 10.69 92.9 Example 4 10.78 93.1 Example 5 10.86 93.2 Example 6 10.76 93.4 Example 7 10.81 92.7 Comparative Example 1 10.77 91.9 Comparative Example 2 10.84 90.8 Comparative Example 3 11.36 91.7 Comparative Example 4 10.05 90.3 Comparative Example 5 11.84 89.8
[0094] Result analysis: Analyze Examples 1-7 and combine the data in Table 2 and Figure 1-2 It can be seen that the coating prepared by the present invention has a fast drying speed in a constant temperature and humidity (35° C., 55%) environment, and can be dried within 10.86 hours; and the glossiness test data at a 60° angle is as high as over 92.7%.
[0095] Analyze Example 1 and Comparative Example 4 and combine the data in Table 2 and Figure 1-2 It can be seen that in the preparation of the composite drying agent, when 12% zirconium isooctanoate is replaced by 8% manganese isooctanoate, the drying effect is improved, and the actual drying speed of the obtained coating in a constant temperature and humidity environment (35°C, 55%) is accelerated, reaching actual drying in 10.05h; however, at the same time, the 60° angle gloss test data decreased significantly, down to 90.3%.
[0096] Analyze Example 1 and Comparative Examples 1, 2, 3 and 5 and combine the data in Table 2 and Figure 1-2 It can be seen that the addition of the nano-silicon modified alkyd resin of the present invention can improve the gloss of the obtained coating; the addition of the composite drying agent of the present invention can also improve the gloss of the obtained coating; and there is a synergistic effect between the two, which can synergistically improve the gloss of the obtained coating. In addition, in the preparation of nano-silicon modified alkyd resin, the introduction of nano-silicon powder is conducive to improving the gloss of the obtained coating; the introduction of nano-silicon powder after organic activation can further improve the gloss of the obtained coating. In the preparation of the composite drying agent, the component 12% zirconium isooctanoate is indispensable. If it is deleted (Comparative Example 3) or replaced (Comparative Example 4), whether the actual drying speed is slowed down (Comparative Example 3) or accelerated (Comparative Example 4), the gloss of the obtained coating will decrease.
[0097] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0098] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A nano-silicon modified resin coating, characterized in that: The raw material components include, by weight: 100 parts of nano-silicon modified alkyd resin, 1-1.4 parts of composite drying agent, 25-30 parts of composite powder filler, 40-45 parts of xylene, 0.6-1 part of dispersant, 0.4-0.7 part of defoamer and 0.3-0.5 part of anti-skinning agent; the nano-silicon modified alkyd resin is prepared by ultrasonically mixing organic nano-silicon and alkyd resin in a mass ratio of 1:40-45.
2. The nano-silicon modified resin coating according to claim 1, characterized in that: The specific preparation method of the nano-silicon modified alkyd resin is as follows: A1. Add organic nano-silicon into alkyd resin, stir at a speed of 100-120r / min for 8-10min to obtain a mixture; A2. The mixture obtained in A1 is subjected to low-frequency ultrasonic treatment for 3-4 hours to obtain nano-silicon modified alkyd resin.
3. The nano-silicon modified resin coating according to claim 1 or 2, characterized in that: Preparation method of organic nano silicon: A11, weigh 25g of nano-silicon powder, disperse it in 750mL of distilled water, stir and heat to 80°C, add 22-25g of 30% by mass hexadecyltrimethylammonium bromide aqueous solution, heat to 90°C, keep constant temperature for 2h, and treat with ultrasonic vibration for 0.5h to obtain the product; A12. Filter the product obtained in A11, wash it with distilled water, let it stand for 12 hours, then filter it again and wash it again. Repeat this process several times until the product is identified as Br free using AgNO3 solution. - Then, put it into a drying oven and dry it at 138-142°C to constant weight to obtain organic nano-silicon.
4. The nano-silicon modified resin coating according to claim 1, characterized in that: The preparation method of the composite drying agent is as follows: 8% cobalt isooctanoate, 8% manganese isooctanoate, 12% zirconium isooctanoate, 5% calcium isooctanoate, 9% zinc isooctanoate and bipyridine are mixed in a mass ratio of 9:5:(5-6):2:1:0.1 and mixed evenly to obtain the composite drying agent.
5. The nano-silicon modified resin coating according to claim 1, characterized in that: The preparation method of the composite powder filler is as follows: B1. Mix heavy calcium powder and light calcium powder in a mass ratio of (2-3):1 to obtain a mixed powder; B2. By weight, 35 parts of the mixed powder obtained from B1 are fed into an activation batching machine, the speed is set to 600-800r / min, the temperature is set to 70-80°C, and then 0.2-0.3 parts of stearate and 0.2-0.3 parts of hydrogen-containing silicone oil are added, the temperature is maintained and stirred for 20-25 minutes to obtain a composite powder filler.
6. The nano-silicon modified resin coating according to claim 1, characterized in that: The dispersant includes BYK-109 dispersant or BYK-164 dispersant.
7. The nano-silicon modified resin coating according to claim 1, characterized in that: The defoamer is EFKA-2526 defoamer.
8. The nano-silicon modified resin coating according to claim 1, characterized in that: The anti-skinning agent is Milliken BNK-DSF1010 anti-skinning agent.
9. A method for preparing a nano-silicon modified resin coating according to any one of claims 1 to 8, characterized in that: The steps include: S1. Put the nano-silicon modified alkyd resin into a disperser, control the stirring speed at 450-500r / min, add a composite drier, a composite powder filler, xylene, a dispersant, a defoamer and an anti-skinning agent, and continue stirring for 15-25min to obtain a primary material; S2. Grind the primary material obtained in S1 to a fineness of no more than 25 μm to obtain a nano-silicon modified resin coating.
Citation Information
Patent Citations
Modified aqueous alkyd resin coating
CN104893519A
Method for dispersing nano silicon
CN110289400A
Single-component water-based asphalt paint for damping spring and preparation method of single-component water-based asphalt paint
CN112409927A
Quick-drying benzene-free alkyd conformal coating and preparation method thereof
CN112608663A
pre-construction Anti-corrosive Primer Paint and forming the coating layer using the same