Colorful-plating thermocuring coating as well as preparation method and application thereof
By using cold-polymerized C9 petroleum resin and a specific rare-earth drier CQ-668, combined with a radiation-crosslinkable organosilicon acrylate leveling agent, the problems of poor color development and poor thermal stability of thermosetting iridescent coatings were solved, achieving excellent drying performance and adhesion, and improving the overall effect of the coating.
Patent Information
- Application Number
- CN202411184024.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-12
AI Technical Summary
Existing thermosetting iridescent coatings suffer from poor color development and thermal stability after coating. In particular, when using conventional rare earth drying agents, the catalytic effect is poor and large amounts need to be added, leading to a decrease in adhesion performance.
The coating composition was optimized to improve drying performance and adhesion by using cold-polymerized C9 petroleum resin and specific rare earth driers (such as CQ-668 from Shanghai Taoyuan Cobalt Co., Ltd.) in combination with radiation-crosslinkable organosilicon acrylate leveling agents, adjusting the ratio of resin and driers, and using a mixed solvent of 200# solvent oil and 120# white spirit.
It achieves normal color development after coating, improves the thermal stability and adhesion of the coating, and ensures that it can maintain excellent drying performance and iridescent coating effect even with low addition amount.
Smart Images

Figure HDA0005013020840000011 
Figure HDA0005013020840000012 
Figure HDA0005013020840000013
Abstract
Description
Technical Field
[0001] The present invention relates to the field of coating technology, in particular to the field of IPCC09D175, and more specifically to a seven-color thermally cured coating and a preparation method and application thereof. Background Art
[0002] Colorful electroplating is a surface treatment technology that forms a colored coating on the metal surface through a specific process. It can make the metal surface present a variety of colors, thereby enhancing the beauty and attractiveness of the product. This technology is not limited to a single color, but can achieve a combination of multiple colors, making the product appearance more diverse and meeting the needs of different consumers. Colorful electroplating has a wide range of applications, including but not limited to the surface treatment of hardware products, aluminum products, hardware, plastic products and other products. This technology can make the product appearance more beautiful and enhance the market competitiveness of the product. The methods for achieving colorful electroplating include but are not limited to chemical nickel plating, surface coloring of electroplated nickel layer, vacuum coating, etc. The addition of different metal activators and the adjustment of parameters such as current and voltage can obtain electroplating layers of different colors and effects, such as gold, silver, bronze, rainbow colors, etc. The matching colorful plating primer needs to take into account adhesion, dryness, hardness, light color and other properties at the same time.
[0003] CN102630655B discloses a colorful fish hook and a method for making the same. The hook is made of a steel fish hook (three-anchor or three-handle hook) as the base hook, and is plated with titanium in the presence of oxygen on the basis of a nickel coating. The manufacturing method is as follows: the steel fish hook is subjected to heat treatment and surface treatment, copper plating, nickel plating, and then titanium plating in an ion plating machine to produce a colorful surface layer. However, the base material used is metal, and multiple electroplatings are performed, so the process is complicated and the base material used is limited. Summary of the invention
[0004] The first aspect of the present invention provides a colorful heat-curing coating, which comprises, by weight, 30-60 parts of alkyd resin, 10-30 parts of petroleum resin, 1-6 parts of rare earth drier, 0.1-1.5 parts of adhesion promoter, and 30-70 parts of solvent.
[0005] The alkyd resin includes at least one of soybean oil modified alkyd resin, polyurethane modified alkyd resin, acrylic acid modified alkyd resin, linseed oil modified alkyd resin, tall oil fatty acid modified alkyd resin and dehydrated castor oil modified alkyd resin.
[0006] The petroleum resin includes at least one of C5 petroleum resin, C9 petroleum resin, C5 / C9 copolymer resin, hydrogenated petroleum resin and coumarone resin.
[0007] The C9 petroleum resin includes cold-polymerized C9 petroleum resin, and the Gardner color scale (ASTM D1544) of the cold-polymerized C9 petroleum resin is 3-6.
[0008] Preferably, the Gardner color scale (ASTM D1544) of the cold-polymerized C9 petroleum resin is 3-5.
[0009] Preferably, the softening point of the C9 petroleum resin (GB / T2294-97) is 110-130°C.
[0010] The present applicant has found that the current heat-cured colorful primer has the disadvantage of poor color development after coating due to the dark color of the resin and the drying agent; the selection of cold-polymerized C9 petroleum resin can solve the problem of dark color development, but the cold-polymerized C9 petroleum resin has a low softening point, resulting in poor thermal stability. The present applicant has further found that the use of rare earth drying agents can improve the thermal stability of the paint film, but the catalytic effect of conventional rare earth drying agents is not as good as that of conventional isooctanoic acid drying agents, resulting in the need to add a large amount of drying agents to improve the drying performance, which will also lead to a decrease in adhesion performance. The present applicant accidentally discovered that the use of Shanghai Taoyuan Cobalt Co., Ltd., Model: CQ-668 rare earth drying agent, can maintain excellent drying performance at a low addition amount and improve adhesion.
[0011] Preferably, the rare earth drier is purchased from Shanghai Taoyuan Cobalt Industry Co., Ltd., model: CQ-668.
[0012] The weight ratio of the petroleum resin to the rare earth drier is (5-10):1.
[0013] Preferably, the weight ratio of the petroleum resin to the rare earth drier is (5-7):1.
[0014] Preferably, the adhesion promoter comprises a radiation-crosslinkable silicone acrylate leveling agent.
[0015] The weight ratio of the alkyd resin to the petroleum resin is (2-3):1.
[0016] Preferably, the weight ratio of the alkyd resin to the petroleum resin is (2-2.5):1.
[0017] The solvent includes a hydrocarbon solvent.
[0018] The hydrocarbon solvent includes at least one of n-heptane, cyclohexane, isooctane, dodecane, white oil, D40 solvent oil, D30 solvent oil, D80 solvent oil, 200# solvent oil, 120# white oil, 100# solvent oil, and 150# solvent oil.
[0019] Preferably, the hydrocarbon solvent includes 200# solvent oil and 120# white spirit, and the weight ratio of the 200# solvent oil to the 120# white spirit is 1:(0.8-1.2).
[0020] The second aspect of the present invention provides a method for preparing a colorful heat-curing coating, comprising the following steps: adding alkyd resin, petroleum resin, rare earth drier, and adhesion promoter into a solvent and stirring evenly to obtain the coating.
[0021] The third aspect of the present invention provides an application of a seven-color heat-curing coating, which is applied to the base coating of plastic blanks.
[0022] Beneficial Effects
[0023] 1. This application uses a specific rare earth drier and cold-polymerized C9 petroleum resin to solve the problem of dark paint film color, thereby achieving normal color development after coating.
[0024] 2. The weight ratio of the petroleum resin to the rare earth drier is (5-10):1, which can further improve the drying performance and thermal stability.
[0025] 3. This application uses the rare earth drier model CQ-668 produced by Shanghai Taoyuan Cobalt Co., Ltd., which can improve adhesion while maintaining excellent drying performance at a low addition amount.
[0026] 4. This application uses a radiation-crosslinkable silicone acrylate leveling agent to further improve the adhesion of the paint film.
[0027] 5. The hydrocarbon solvent includes 200# solvent oil and 120# white oil, and the weight ratio of the 200# solvent oil to the 120# white oil is 1:(0.8-1.2), which can further improve the colorful plating effect after coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is the colorful plating effect obtained by the primer in Example 1.
[0029] Figure 2 This is the colorful plating effect obtained by the primer in Example 2.
[0030] Figure 3 This is the colorful plating effect obtained by the primer in Example 3.
[0031] Figure 4 This is the colorful plating effect obtained by the primer in Example 4.
[0032] Figure 5 This is the colorful plating effect obtained by the primer in Example 5. DETAILED DESCRIPTION
[0033] Example 1
[0034] A colorful heat-curing coating comprises, by weight, 40 parts of alkyd resin, 18 parts of petroleum resin, 3 parts of rare earth drier, 0.5 parts of adhesion promoter and 49 parts of solvent.
[0035] The solvent is 24 parts of 200# solvent oil and 25 parts of 120# white spirit, both of which are general-purpose commercially available solvents, regardless of the manufacturer.
[0036] The alkyd resin is soybean oil modified alkyd resin purchased from Henan Aohui Industrial Coatings Co., Ltd.
[0037] The petroleum resin is thermally polymerized 8#C9 petroleum resin purchased from Puyang Hengtai Petrochemical, model T1120.
[0038] The rare earth drier is CQ-668 from Shanghai Taoyuan Cobalt Co., Ltd.
[0039] The adhesion promoter is TEGO-2100 silicone acrylate leveling agent.
[0040] A preparation method of a seven-color heat-curing coating comprises the following steps: adding alkyd resin, petroleum resin, rare earth drier and adhesion promoter into a solvent and stirring the mixture evenly to obtain the coating.
[0041] Example 2
[0042] A colorful heat-curing coating comprises, by weight, 40 parts of alkyd resin, 18 parts of petroleum resin, 3 parts of rare earth drier, 0.5 parts of adhesion promoter and 49 parts of solvent.
[0043] The solvent is 24 parts of 200# solvent oil and 25 parts of 120# white spirit, both of which are general-purpose commercially available solvents, regardless of the manufacturer.
[0044] The alkyd resin is soybean oil modified alkyd resin purchased from Henan Aohui Industrial Coatings Co., Ltd.
[0045] The petroleum resin is thermally polymerized 14#C9 petroleum resin purchased from Puyang Hengtai Petrochemical, model T1130.
[0046] The rare earth drier is CQ-668 from Shanghai Taoyuan Cobalt Co., Ltd.
[0047] The adhesion promoter is TEGO-2100 silicone acrylate leveling agent.
[0048] A preparation method of a seven-color heat-curing coating comprises the following steps: adding alkyd resin, petroleum resin, rare earth drier and adhesion promoter into a solvent and stirring the mixture evenly to obtain the coating.
[0049] Example 3
[0050] A colorful heat-curing coating comprises, by weight, 40 parts of alkyd resin, 18 parts of petroleum resin, 3 parts of rare earth drier, 0.5 parts of adhesion promoter and 49 parts of solvent.
[0051] The solvent is 24 parts of 200# solvent oil and 25 parts of 120# white spirit, both of which are general-purpose commercially available solvents, regardless of the manufacturer.
[0052] The alkyd resin is soybean oil modified alkyd resin purchased from Henan Aohui Industrial Coatings Co., Ltd.
[0053] The petroleum resin is cold-polymerized C9 petroleum resin purchased from Puyang Hengtai Petrochemical.
[0054] The rare earth drier is CQ-668 from Shanghai Taoyuan Cobalt Co., Ltd.
[0055] The adhesion promoter is TEGO-2100 silicone acrylate leveling agent.
[0056] A preparation method of a seven-color heat-curing coating comprises the following steps: adding alkyd resin, petroleum resin, rare earth drier and adhesion promoter into a solvent and stirring the mixture evenly to obtain the coating.
[0057] Example 4
[0058] A colorful heat-curing coating comprises, by weight, 40 parts of alkyd resin, 18 parts of petroleum resin, 3 parts of drying agent, 0.5 parts of adhesion promoter and 49 parts of solvent.
[0059] The solvent is 24 parts of 200# solvent oil and 25 parts of 120# white spirit, both of which are general-purpose commercially available solvents, regardless of the manufacturer.
[0060] The alkyd resin is soybean oil modified alkyd resin purchased from Henan Aohui Industrial Coatings Co., Ltd.
[0061] The petroleum resin is thermally polymerized 8#C9 petroleum resin purchased from Puyang Hengtai Petrochemical, model T1120.
[0062] The drier is 2-ethylhexanoic acid drier purchased from Shandong Lingsai Coatings Co., Ltd. The metal content of the 2-ethylhexanoic acid composite drier is 8%.
[0063] The adhesion promoter is TEGO-2100 silicone acrylate leveling agent.
[0064] A preparation method of a seven-color heat-curing coating comprises the following steps: adding alkyd resin, petroleum resin, rare earth drier and adhesion promoter into a solvent and stirring the mixture evenly to obtain the coating.
[0065] Example 5
[0066] A colorful heat-curing coating comprises, by weight, 40 parts of alkyd resin, 18 parts of petroleum resin, 3 parts of rare earth drier, 0.5 parts of adhesion promoter and 49 parts of solvent.
[0067] The solvent is 24 parts of 200# solvent oil and 25 parts of 120# white spirit, both of which are general-purpose commercially available solvents, regardless of the manufacturer.
[0068] The alkyd resin is soybean oil modified alkyd resin purchased from Henan Aohui Industrial Coatings Co., Ltd.
[0069] The petroleum resin is thermally polymerized 8#C9 petroleum resin purchased from Puyang Hengtai Petrochemical, model T1120.
[0070] The rare earth drier was purchased from Wenzhou Shoucheng Chemical Technology Co., Ltd.
[0071] The adhesion promoter is TEGO-2100 silicone acrylate leveling agent.
[0072] A preparation method of a seven-color heat-curing coating comprises the following steps: adding alkyd resin, petroleum resin, rare earth drier and adhesion promoter into a solvent and stirring the mixture evenly to obtain the coating.
[0073] Performance Testing Methods and Data
[0074] The primer prepared in the example was sprayed on the ABS plastic blank with a thickness of 30±5 um and baked at 70°C for 3 hours in a well-ventilated and oxygen-supplied environment.
[0075] 1. Adhesion test: The picture shows the effect of seven-color plating after roller coating. (No topcoat is required) The test method is a hundred-grid test, specifically GB / T9286-1998 "Scratch test of paint and varnish film", ASTMD3359-2002 "Adhesion determination by tape method", ISO2409-2007 "Paint and varnish-scratch test", and the adhesion reaches 4B~5B.
[0076] 2. Drying performance: The conventional drying performance is that after the colorful plating, the colorful effect of the paint surface has not changed after being placed at room temperature (25℃~28℃) for three months. The factory test standard is to roll the primer, bake at 50℃ for 3 hours, and after the colorful plating, bake in an 80℃ oven for half an hour, and the colorful effect of the paint surface has not changed.
[0077] 3. The colorful plating effect is as follows Figure 1-5As shown, Example 3 uses cold-polymerized petroleum resin and CQ-668 rare earth drier to obtain a colorful plating effect with a light paint film and good color development; Example 1 uses a light-colored hot-polymerized petroleum resin and a rare earth drier to obtain a colorful plating effect with a light paint film and good color development, but the color is slightly yellower than the cold-polymerized petroleum resin; Example 2 uses a dark-colored hot-polymerized petroleum resin and a rare earth drier, the paint film color is heavy, and the colorful plating has obvious poor color development; Example 4 uses a light-colored hot-polymerized petroleum resin and isooctonic acid drier, the paint film color is heavy, and the colorful plating has poor color development; Example 5 uses cold-polymerized petroleum resin and other brands of rare earth driers to obtain a colorful plating effect with a light paint film and good color development, but the catalytic effect of the control rare earth drier is not as good as that of Experimental Example 3. Under the same temperature and time drying environment, the actual drying degree of the paint film is relatively poor, it is easy to not dry, and the paint film is soft.
Claims
1. A colorful heat-curing coating, characterized in that: The components include, by weight: 30-60 parts of alkyd resin, 10-30 parts of petroleum resin, 1-6 parts of rare earth drier, 0.1-1.5 parts of adhesion promoter and 30-70 parts of solvent.
2. The seven-color thermal curing coating according to claim 1, characterized in that: The alkyd resin includes at least one of soybean oil modified alkyd resin, polyurethane modified alkyd resin, acrylic acid modified alkyd resin, linseed oil modified alkyd resin, tall oil fatty acid modified alkyd resin and dehydrated castor oil modified alkyd resin.
3. The seven-color thermal curing coating according to claim 2 is characterized in that: The petroleum resin includes at least one of C5 petroleum resin, C9 petroleum resin, C5 / C9 copolymer resin, hydrogenated petroleum resin and coumarone resin.
4. The seven-color thermal curing coating according to claim 3 is characterized in that: The C9 petroleum resin includes cold-polymerized C9 petroleum resin, and the Gardner color scale of the cold-polymerized C9 petroleum resin is 3-6.
5. The seven-color thermal curing coating according to claim 4 is characterized in that: The softening point of the C9 petroleum resin is 110-130°C.
6. The seven-color thermal curing coating according to claim 1, characterized in that: The adhesion promoter includes a radiation-crosslinkable silicone acrylate leveling agent.
7. The seven-color thermal curing coating according to claim 6, characterized in that: The weight ratio of the alkyd resin to the petroleum resin is (2-3):
1.
8. The seven-color thermal curing coating according to claim 1, characterized in that: The solvent includes a hydrocarbon solvent.
9. A method for preparing the colorful heat-curing coating according to any one of claims 1 to 8, characterized in that: The following steps are involved: Add alkyd resin, petroleum resin, rare earth drier and adhesion promoter into the solvent and stir evenly.
10. An application of the seven-color thermal curing coating according to any one of claims 1 to 8, characterized in that: Used for base coating of plastic blanks.
Citation Information
Patent Citations
Bottom surface universal type alkyd antirust paint and preparation method thereof
CN106280932A
Method for preparing conformal coating by using rare earth drier
CN117866517A