Environment-friendly green coating simulating plant spectral reflection curve as well as preparation method and application of environment-friendly green coating

Through environmentally friendly green paints imitating the spectral reflection curve of plants, using environmentally friendly materials such as aqueous polymer resin and cobalt green, the problem that existing camouflage paints cannot simulate the spectral reflection characteristics of green vegetation and contain toxic substances is solved, and hyperspectral imaging is achieved Effective camouflage and environmentally friendly coating applications.

CN118931345APending Publication Date: 2024-11-12陕西华秦科技实业股份有限公司

Patent Information

Application Number
CN202410498004.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-04-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing camouflage paints cannot effectively simulate the spectral reflection characteristics of green vegetation in the 600-900nm band, and also contain toxic and harmful substances, such as chromium yellow and lead chromium yellow, resulting in environmental pollution and health hazards.

Method used

Environmentally friendly green coatings that imitate plant spectral reflection curves are used to prepare environmentally friendly coatings without lead-chromium compounds through the combination of aqueous polymer resin, cobalt green and other pigments, combined with aqueous additives, to prepare environmentally friendly coatings without lead-chromium compounds, which meet the 600-900nm band. Spectral reflective properties and are applied to the target surface by spraying or coating.

Benefits of technology

It realizes effective camouflage for hyperspectral imaging detection, fully simulates the spectral reflection characteristics of green vegetation, and avoids the use of toxic substances, meets national environmental protection requirements, and ensures human health and environmental safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931345A_ABST
    Figure CN118931345A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of functional coatings, and relates to an environment-friendly green coating as well as a preparation method and application thereof, in particular to an environment-friendly green coating simulating a plant spectral reflection curve as well as a preparation method and application thereof. The water-based polymer resin and other auxiliaries adopted by the invention are water-based environment-friendly compounds, do not contain toxic and harmful substances and are harmless to human bodies; the adopted pigment does not contain lead and chromium compounds, is environment-friendly and healthy, and meets the national environmental protection requirements; and secondly, the spectral reflection characteristic of cobalt green in the wave band of 600-900nm is closest to the spectral reflection characteristic of green vegetation, so that the environment-friendly green coating prepared by the invention can simulate the spectral reflection characteristic of the green vegetation in the wave band of 600-900nm by compounding cobalt green with other pigments, and can effectively resist hyperspectral imaging detection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of functional coatings, and relates to an environmentally friendly green coating, a preparation method and an application thereof, and specifically relates to an environmentally friendly green coating with a plant spectral reflectance curve, a preparation method and an application thereof. Background Art

[0002] In recent years, with the rapid development of science and technology, the continuous application and popularization of modern remote sensing detection technology, especially hyperspectral imaging technology, in various fields, the requirements for camouflage materials and camouflage effects used in important facilities and equipment are becoming higher and higher. Among them, due to the advantages of low cost, easy use, simple operation, and no restrictions on the shape of parts, coatings have become the fastest-growing and most studied camouflage materials in recent years.

[0003] When using paint to camouflage facilities and equipment, it is necessary to ensure that the ratio K of the average spectral reflectance of the near-infrared band (710-880nm) and the red light region (620-660nm) of the camouflaged target is not less than 5, and at the same time, the spectral reflectance channel requirements of green vegetation chlorophyll in the 600-900nm band are met to meet the camouflage protection requirements. However, the commonly used camouflage paints can only meet the requirements in terms of color, or form a "green reflection peak" in the 550nm band and a "red edge" in the 680-740nm spectral reflectance, so it cannot 100% simulate the spectral reflectance characteristics of green vegetation in the 600-900nm band.

[0004] In addition, common green paints use oily resins as film-forming substances and organic solvents as solvents. Pigments are often formulated with compounds containing chromium and lead (chrome yellow, lead chrome yellow). The resulting camouflage paints contain more toxic and harmful substances, which seriously endanger human health and cause great pollution to the environment.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide an environmentally friendly green paint that imitates the spectral reflectance curve of plants and its preparation method and application. After using the paint for camouflage, it can meet the spectral reflectance characteristics of the band between 600 and 900 nm and meet national environmental protection requirements.

[0007] To achieve the above object, the present invention provides the following technical solutions:

[0008] On the one hand, the present invention provides an environmentally friendly green coating imitating a plant spectral reflectance curve, comprising a component A and a component B, wherein the weight ratio of the component A to the component B is A:B=(40-80):1;

[0009] The component A comprises the following components by weight: 35-45 parts of water-based polymer resin, 30-40 parts of pigment, 10-15 parts of first component water, 0.5-2 parts of water-based defoamer, 0.5-2 parts of water-based wetting agent, 1-2 parts of moisturizer, 1-10 parts of water-based dispersant, 1-3 parts of talc, and 1-4 parts of water-based light stabilizer;

[0010] The B component includes the following components by weight: 80-90 parts of curing agent and 10-20 parts of the second component water;

[0011] The pigments include cobalt green and other pigments, and the other pigments are one or more of chrome green, iron yellow, iron red, composite titanium yellow, composite titanium red, zinc yellow, cobalt blue, titanium chrome brown, molybdenum chrome red, and organic yellow.

[0012] Specifically, the water-based polymer resin includes but is not limited to any one or more of polyurethane resin, epoxy resin, and acrylic resin.

[0013] Specifically, the pigment comprises the following components by weight: 15 to 70 parts of cobalt green and 30 to 85 parts of other pigments.

[0014] Specifically, the curing agent is a water-based blocked isocyanate curing agent.

[0015] On the other hand, the present invention provides a method for preparing the environmentally friendly green coating having the plant spectral reflectance curve as described above, wherein component A and component B are prepared separately, and then component A and component B are mixed and stirred evenly to prepare the environmentally friendly green coating;

[0016] The preparation of the A component specifically includes:

[0017] Step 1, adding the first component of water, aqueous defoamer, aqueous wetting agent and cobalt green in the pigment into a mixing container, and stirring for the first time until the mixture is uniform, to obtain a mixture a;

[0018] Step 2, adding other pigments, aqueous dispersants, moisturizers and talcum powder to mixture a, stirring for a second time until the mixture is uniformly mixed; then grinding, and transferring the mixture to a mixing container after grinding is uniform, to obtain mixture b;

[0019] Step 3: Add water-based polymer resin and water-based light stabilizer to mixture b, and stir for a third time until the mixture is evenly mixed to obtain component A of the environmentally friendly green coating.

[0020] Specifically, the preparation of the B component specifically includes:

[0021] Add the curing agent and the second component water into a new mixing container and stir for the fourth time until they are evenly mixed to obtain component B of the environmentally friendly green coating; the stirring speed of the fourth stirring is 500-600 r / min, and the stirring time is 2-5 min.

[0022] Specifically, in step 1, the stirring speed of the first stirring is 500-800 r / min, and the stirring time is 5-10 min.

[0023] Specifically, in step 2, the stirring speed of the second stirring is 800-1000 r / min, and the stirring time is 10-15 min; the grinding speed is 1800-2200 r / min, and the grinding time is 60-120 min.

[0024] Specifically, in step 3, the stirring speed of the third stirring is 1000-1200 r / min, and the stirring time is 10-20 min.

[0025] On the other hand, the present invention provides an application of the environmentally friendly green paint as described above, wherein the environmentally friendly green paint is sprayed or coated to form a coating on the surface of the target to be camouflaged, so as to completely simulate the spectral reflectance characteristics of green vegetation in the 600-900nm band.

[0026] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects:

[0027] The water-based polymer resin and other additives used in the present invention are all water-based environmentally friendly compounds, do not contain toxic and harmful substances and are harmless to the human body; the pigment used does not contain lead and chromium compounds, is environmentally friendly and healthy, and meets national environmental protection requirements;

[0028] Secondly, since the spectral reflectance characteristics of cobalt green in the 600-900nm band are closest to the spectral reflectance characteristics of green vegetation, the environmentally friendly green paint prepared by the present invention can simulate the spectral reflectance characteristics of green vegetation in the 600-900nm band by compounding cobalt green with other pigments, and effectively resist hyperspectral imaging detection. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] The accompanying drawings are incorporated in and constitute a part of this specification and, together with the description, serve to explain the principles of the present invention.

[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0031] Figure 1 A spectral reflection curve diagram of an environmentally friendly green coating prepared according to an embodiment of the present invention;

[0032] Figure 2 The present invention is a flow chart of the method for preparing the coating. DETAILED DESCRIPTION

[0033] Here, exemplary embodiments will be described in detail, and examples thereof are shown in the accompanying drawings. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present invention. Instead, they are only examples consistent with some aspects of the present invention as detailed in the appended claims.

[0034] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.

[0035] Example 1

[0036] This embodiment provides an environmentally friendly green paint that imitates the spectral reflectance curve of plants, which includes the following components and proportions by weight:

[0037] Component A: 40 parts by weight of water-based aliphatic polyurethane resin, 34 parts by weight of pigment (including 20 parts by weight of cobalt green, 12 parts by weight of titanium chrome yellow, 29 parts by weight of cobalt blue, and 39 parts by weight of organic yellow), 12 parts by weight of the first component of water, 1 part by weight of water-based defoamer, 1 part by weight of water-based wetting agent, 2 parts by weight of moisturizer, 8 parts by weight of water-based dispersant, 3 parts by weight of talc, and 2 parts by weight of water-based light stabilizer;

[0038] Component B: 85 parts by weight of water-based blocked isocyanate (curing agent), and 15 parts by weight of the second component water; wherein component A: component B = 80:1.

[0039] The preparation process is as follows: (1) adding the first component of water, aqueous defoamer, aqueous wetting agent and cobalt green into a mixing kettle and stirring for 8 minutes at a speed of 600 r / min until the above substances are evenly mixed;

[0040] (2) adding other pigments except cobalt green, aqueous dispersant, moisturizer and talcum powder to the mixture, stirring at a speed of 1000 r / min for 10 minutes, and then pouring into a sand mill and grinding at a speed of 2000 r / min for 60 minutes;

[0041] (3) After grinding, pour it back into the mixing kettle, add water-based aliphatic polyurethane resin and water-based light stabilizer, and stir at a speed of 1100 r / min for 15 minutes to obtain component A of the environmentally friendly green coating;

[0042] (4) Add the curing agent and the second component water into a new mixing kettle and stir at a speed of 500 r / min for 3 minutes to obtain component B of the environmentally friendly green coating.

[0043] Component A and component B are mixed according to the mass ratio to finally obtain an environmentally friendly green paint with a plant-like spectral reflectance curve, the ratio of the average spectral reflectance of the near-infrared band (710-880nm) and the red light region (620-660nm) is K1=6.06, see Figure 1 shown.

[0044] Example 2

[0045] This embodiment provides an environmentally friendly green paint that imitates the spectral reflectance curve of plants, which includes the following components and proportions by weight:

[0046] Component A: 42 parts by weight of water-based aliphatic polyurethane resin, 35 parts by weight of pigment (including 21 parts by weight of cobalt green, 32 parts by weight of chrome green, 4 parts by weight of iron oxide red, 13 parts by weight of cobalt blue, and 30 parts by weight of organic yellow), 13 parts by weight of the first component of water, 1 part by weight of water-based defoamer, 1 part by weight of water-based wetting agent, 2 parts by weight of moisturizer, 2 parts by weight of water-based dispersant, 2 parts by weight of talc, and 2 parts by weight of water-based light stabilizer;

[0047] Component B: 85 parts by weight of water-based blocked isocyanate (curing agent), and 15 parts by weight of the second component water; wherein component A: component B = 60:1.

[0048] See also Figure 2 As shown, the preparation process is as follows: (1) adding the first component of water, aqueous defoamer, aqueous wetting agent, and cobalt green into a mixing kettle and stirring for 10 minutes at a speed of 500 r / min until the above substances are evenly mixed;

[0049] (2) adding other pigments except cobalt green, aqueous dispersant, moisturizer and talcum powder to the mixture, stirring at a speed of 800 r / min for 15 minutes, and then pouring into a sand mill and grinding at a speed of 1900 r / min for 90 minutes;

[0050] (3) After grinding, pour it back into the mixing kettle, add water-based aliphatic polyurethane resin and water-based light stabilizer, and stir at a speed of 1000 r / min for 20 minutes to obtain component A of the environmentally friendly green coating;

[0051] (4) Add the curing agent and the second component water into a mixing kettle and stir for 3 minutes at a speed of 600 r / min to obtain component B of the environmentally friendly green coating.

[0052] Component A and component B are mixed according to the mass ratio to finally obtain an environmentally friendly green paint with a plant-like spectral reflectance curve, the ratio of the average spectral reflectance of the near-infrared band (710-880nm) and the red light region (620-660nm) is K2=7.73, see Figure 1 shown.

[0053] Example 3

[0054] This embodiment provides an environmentally friendly green paint that imitates the spectral reflectance curve of plants, which includes the following components and proportions by weight:

[0055] Component A: 38 parts by weight of aqueous acrylic resin, 38 parts by weight of pigment (including 28 parts by weight of cobalt green, 6 parts by weight of cobalt blue, and 67 parts by weight of organic yellow), 10 parts by weight of the first component of water, 1 part by weight of aqueous defoamer, 1 part by weight of aqueous wetting agent, 2 parts by weight of moisturizer, 10 parts by weight of aqueous dispersant, 2 parts by weight of talc, and 2 parts by weight of aqueous light stabilizer;

[0056] Component B: 80 parts by weight of water-based blocked isocyanate (curing agent), and 20 parts by weight of the second component water; wherein component A: component B = 70:1.

[0057] See also Figure 2 As shown, the preparation process is as follows: (1) adding the first component of water, aqueous defoamer, aqueous wetting agent, and cobalt green into a mixing kettle and stirring for 10 minutes at a speed of 600 r / min until the above substances are evenly mixed;

[0058] (2) adding other pigments except cobalt green, aqueous dispersant, moisturizer and talcum powder to the mixture, stirring at a speed of 800 r / min for 12 minutes, and then pouring into a sand mill and grinding at a speed of 2000 r / min for 60 minutes;

[0059] (3) After grinding, pour it back into the mixing kettle, add water-based acrylic resin and water-based light stabilizer, and stir at a speed of 1000 r / min for 15 minutes to obtain component A of the environmentally friendly green coating;

[0060] (4) Add the curing agent and the second component water into a mixing kettle and stir for 5 minutes at a speed of 500 r / min to obtain component B of the environmentally friendly green coating.

[0061] Component A and component B are mixed according to the mass ratio to finally obtain an environmentally friendly green paint with a plant-like spectral reflectance curve, the ratio of the average spectral reflectance of the near-infrared band (710-880nm) and the red light region (620-660nm) is K3=6.23, see Figure 1 shown.

[0062] Example 4

[0063] The present embodiment provides an environmentally friendly green paint that imitates a plant spectral reflectance curve, which includes the following components and proportions by weight.

[0064] Component A: 45 parts by weight of water-based acrylic resin, 36 parts by weight of pigment (including 35 parts by weight of cobalt green, 5 parts by weight of chrome green, 9 parts by weight of iron red, 24 parts by weight of cobalt blue, and 27 parts by weight of organic yellow), 14 parts by weight of the first component of water, 1 part by weight of water-based defoamer, 1 part by weight of water-based wetting agent, 2 parts by weight of moisturizer, 2 parts by weight of water-based dispersant, 2 parts by weight of talc, and 2 parts by weight of water-based light stabilizer;

[0065] Component B: 90 parts by weight of water-based blocked isocyanate (curing agent), and 10 parts by weight of the second component water; wherein component A: component B = 80:1.

[0066] See also Figure 2 As shown, the preparation process is as follows: (1) adding the first component of water, aqueous defoamer, aqueous wetting agent, and cobalt green into a mixing kettle and stirring for 10 minutes at a speed of 600 r / min until the above substances are evenly mixed;

[0067] (2) adding other pigments except cobalt green, aqueous dispersant, moisturizer and talcum powder to the mixture, stirring at a speed of 900 r / min for 10 minutes, and then pouring into a sand mill and grinding at a speed of 1900 r / min for 80 minutes;

[0068] (3) After grinding, pour it back into the mixing kettle, add water-based acrylic resin and water-based light stabilizer, and stir at a speed of 1100 r / min for 12 minutes to obtain component A of the environmentally friendly green coating;

[0069] (4) Add the curing agent and the second component water into a mixing kettle and stir at a speed of 550 r / min for 5 minutes to obtain component B of the environmentally friendly green coating.

[0070] Component A and component B are mixed according to the mass ratio to finally obtain an environmentally friendly green paint with a plant-like spectral reflectance curve, the ratio of the average spectral reflectance of the near-infrared band (710-880nm) and the red light region (620-660nm) is K4=5.98, see Figure 1 shown.

[0071] Example 5

[0072] The present embodiment provides an environmentally friendly green paint that imitates a plant spectral reflectance curve, which includes the following components and proportions by weight.

[0073] Component A: 36 parts by weight of water-based epoxy resin, 40 parts by weight of pigment (including 40 parts by weight of cobalt green, 5 parts by weight of composite titanium red, 35 parts by weight of cobalt blue, 20 parts by weight of composite titanium yellow), 10 parts by weight of the first component of water, 1 part by weight of water-based defoamer, 1 part by weight of water-based wetting agent, 2 parts by weight of moisturizer, 2 parts by weight of water-based dispersant, 2 parts by weight of talc, and 2 parts by weight of water-based light stabilizer;

[0074] Component B: 85 parts by weight of water-based blocked isocyanate (curing agent), 15 parts by weight of the second component water; wherein component A: component B = 55:1.

[0075] See also Figure 2 As shown, the preparation process is as follows: (1) adding water, aqueous defoamer, aqueous wetting agent and cobalt green into a mixing kettle and stirring for 10 minutes at a speed of 500 r / min until the above substances are evenly mixed;

[0076] (2) adding other pigments except cobalt green, aqueous dispersant, moisturizer and talcum powder to the mixture, stirring at a speed of 1000 r / min for 10 minutes, and then pouring into a sand mill and grinding at a speed of 2000 r / min for 70 minutes;

[0077] (3) After grinding, pour it back into the mixing kettle, add water-based epoxy resin and water-based light stabilizer, and stir at a speed of 1200 r / min for 10 minutes to obtain component A of the environmentally friendly green coating;

[0078] (4) Add the curing agent and the second component water into a mixing kettle and stir at a speed of 600 r / min for 5 minutes to obtain component B of the environmentally friendly green coating.

[0079] Component A and component B are mixed according to the mass ratio to finally obtain an environmentally friendly green paint with a plant-like spectral reflectance curve, the ratio of the average spectral reflectance of the near-infrared band (710-880nm) and the red light region (620-660nm) is K5=5.13, see Figure 1 shown.

[0080] Example 6

[0081] The present embodiment provides an environmentally friendly green paint that imitates a plant spectral reflectance curve, which includes the following components and proportions by weight.

[0082] Component A: 40 parts by weight of water-based epoxy resin, 38 parts by weight of pigment (including 35 parts by weight of cobalt green, 5 parts by weight of chrome green, 9 parts by weight of iron red, 24 parts by weight of cobalt blue, and 27 parts by weight of organic yellow), 10 parts by weight of the first component of water, 1 part by weight of water-based defoamer, 1 part by weight of water-based wetting agent, 2 parts by weight of moisturizer, 3 parts by weight of water-based dispersant, 3 parts by weight of talc, and 2 parts by weight of water-based light stabilizer;

[0083] Component B: 80 parts by weight of water-based blocked isocyanate (curing agent), and 20 parts by weight of the second component water; wherein component A: component B = 80:1.

[0084] See also Figure 2 As shown, the preparation process is as follows: (1) adding the first component of water, aqueous defoamer, aqueous wetting agent, and cobalt green into a mixing kettle and stirring for 5 minutes at a speed of 500 r / min until the above substances are evenly mixed;

[0085] (2) adding other pigments except cobalt green, aqueous dispersant, moisturizer and talcum powder to the mixture, stirring at a speed of 900 r / min for 13 minutes, and then pouring into a sand mill and grinding at a speed of 1800 r / min for 70 minutes;

[0086] (3) After grinding, pour it back into the mixing kettle, add water-based epoxy resin and water-based light stabilizer, and stir at a speed of 1100 r / min for 12 minutes to obtain component A of the environmentally friendly green coating;

[0087] (4) Add the curing agent and the second component water into a mixing kettle and stir at a speed of 500 r / min for 2 minutes to obtain component B of the environmentally friendly green coating.

[0088] Component A and component B are mixed according to the mass ratio to finally obtain an environmentally friendly green paint with a plant-like spectral reflectance curve, the ratio of the average spectral reflectance of the near-infrared band (710-880nm) and the red light region (620-660nm) is K6=6.99, see Figure 1 shown.

[0089] Example 7

[0090] The present embodiment provides an environmentally friendly green paint that imitates a plant spectral reflectance curve, which includes the following components and proportions by weight.

[0091] Component A: 36 parts by weight of water-based epoxy resin, 40 parts by weight of pigment (70 parts by weight of cobalt green, 30 parts by weight of titanium chrome brown), 12 parts by weight of first component water, 1 part by weight of water-based defoamer, 1 part by weight of water-based wetting agent, 2 parts by weight of moisturizer, 3 parts by weight of water-based dispersant, 3 parts by weight of talc, 2 parts by weight of water-based light stabilizer;

[0092] Component B: 85 parts by weight of water-based blocked isocyanate (curing agent), 15 parts by weight of the second component water; wherein component A: component B = 40:1.

[0093] See also Figure 2As shown, the preparation process is as follows: (1) adding the first component of water, aqueous defoamer, aqueous wetting agent, and cobalt green into a mixing kettle and stirring for 6 minutes at a speed of 600 r / min until the above substances are evenly mixed;

[0094] (2) adding other pigments except cobalt green, aqueous dispersant, moisturizer and talcum powder to the mixture, stirring at a speed of 100 r / min for 12 minutes, and then pouring into a sand mill and grinding at a speed of 2000 r / min for 60 minutes;

[0095] (3) pouring the mixture back into the mixing kettle, adding water-based epoxy resin and water-based light stabilizer, stirring at a speed of 1100 r / min for 15 minutes, and obtaining component A of the environmentally friendly green coating;

[0096] (4) Add the curing agent and the second component water into a mixing kettle and stir for 5 minutes at a speed of 500 r / min to obtain component B of the environmentally friendly green coating.

[0097] Component A and component B are mixed according to the mass ratio to finally obtain an environmentally friendly green paint with a plant-like spectral reflectance curve, the ratio of the average spectral reflectance of the near-infrared band (710-880nm) and the red light region (620-660nm) is K7=6.31, see Figure 1 shown.

[0098] The present invention provides an environmentally friendly green paint that imitates the plant spectral reflection curve. The spectral reflection characteristics in the 600-900nm band can 100% simulate the spectral characteristics of green vegetation. The raw materials used in the present invention do not contain toxic and harmful substances such as lead chromium compounds and organic solvents. The paint is environmentally friendly and healthy, has no pollution to the environment, and meets national environmental protection requirements.

[0099] The above description is only a specific embodiment of the present invention, so that those skilled in the art can understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention.

[0100] It should be understood that the present invention is not limited to what has been described above and that various modifications and changes may be made without departing from its scope. The scope of the present invention is limited only by the appended claims.

Claims

1. An environmentally friendly green paint imitating the plant spectral reflectance curve, characterized in that: It comprises a component A and a component B, wherein the weight ratio of the component A to the component B is A:B=(40-80):1; The component A comprises the following components by weight: 35-45 parts of water-based polymer resin, 30-40 parts of pigment, 10-15 parts of first component water, 0.5-2 parts of water-based defoamer, 0.5-2 parts of water-based wetting agent, 1-2 parts of moisturizer, 1-10 parts of water-based dispersant, 1-3 parts of talc, and 1-4 parts of water-based light stabilizer; The B component includes the following components by weight: 80-90 parts of curing agent and 10-20 parts of the second component water; The pigments include cobalt green and other pigments, and the other pigments are one or more of chrome green, iron yellow, iron red, composite titanium yellow, composite titanium red, zinc yellow, cobalt blue, titanium chrome brown, molybdenum chrome red, and organic yellow.

2. The environmentally friendly green coating according to claim 1, characterized in that: The waterborne polymer resin includes, but is not limited to, any one or more of polyurethane resin, epoxy resin, and acrylic resin.

3. The environmentally friendly green coating according to claim 1, characterized in that: The pigment comprises the following components by weight: 15 to 70 parts of cobalt green and 30 to 85 parts of other pigments.

4. The environmentally friendly green coating according to claim 1, characterized in that: The curing agent is a water-based blocked isocyanate curing agent.

5. A method for preparing an environmentally friendly green coating based on the plant-mimicking spectral reflectance curve according to any one of claims 1 to 4, characterized in that: Prepare component A and component B respectively, then mix and stir component A and component B evenly to prepare an environmentally friendly green coating; The preparation of the A component specifically includes: Step 1, adding the first component of water, aqueous defoamer, aqueous wetting agent and cobalt green in the pigment into a mixing container, and stirring for the first time until the mixture is uniform, to obtain a mixture a; Step 2, adding other pigments, aqueous dispersants, moisturizers and talcum powder to mixture a, stirring for a second time until the mixture is uniformly mixed; then grinding, and transferring the mixture to a mixing container after grinding is uniform, to obtain mixture b; Step 3: Add water-based polymer resin and water-based light stabilizer to mixture b, and stir for a third time until the mixture is evenly mixed to obtain component A of the environmentally friendly green coating.

6. The method for preparing the environmentally friendly green coating according to claim 5, characterized in that: The preparation of the B component specifically includes: Add the curing agent and the second component water into a new mixing container and stir for the fourth time until they are evenly mixed to obtain component B of the environmentally friendly green coating; the stirring speed of the fourth stirring is 500-600 r / min, and the stirring time is 2-5 min.

7. The method for preparing the environmentally friendly green coating according to claim 5, characterized in that: In step 1, the stirring speed of the first stirring is 500-800 r / min, and the stirring time is 5-10 min.

8. The method for preparing the environmentally friendly green coating according to claim 5, characterized in that: In step 2, the stirring speed of the second stirring is 800-1000 r / min, and the stirring time is 10-15 min; the grinding speed is 1800-2200 r / min, and the grinding time is 60-120 min.

9. The method for preparing the environmentally friendly green coating according to claim 5, characterized in that: In step 3, the stirring speed of the third stirring is 1000-1200 r / min, and the stirring time is 10-20 min.

10. An application of the environmentally friendly green coating according to any one of claims 1 to 4, characterized in that: The environmentally friendly green paint is sprayed or coated to form a coating on the surface of the target to be camouflaged, so as to completely simulate the spectral reflection characteristics of green vegetation in the 600-900nm band.

Citation Information

Patent Citations

  • Environment-friendly paint simulating hyperspectrum of green vegetation and preparation method of environment-friendly paint

    CN103436151A

  • Preparation of green optical and near-infrared camouflage covering cloth

    CN115434155A

  • Water-based two-component typical green optical camouflage coating as well as preparation and coating methods thereof

    CN115806768A

  • Hyperspectral green color paste and preparation method thereof

    CN116218286A

Cited By

  • Vegetation-imitated visible-near infrared camouflage coating as well as preparation method and application thereof

    CN120041025A