Water-based finishing varnish as well as preparation method and application thereof
Through the combination of aqueous hydroxyacrylate and polyurethane dispersions with different glass transition temperatures, the difficulty of water-based varnish is solved in the construction of extreme environments, and the coating effect with high adhesion and gloss is achieved. It is suitable for rail transit vehicles painted.
Patent Information
- Application Number
- CN202410990953.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
When existing water-based cover varnish is constructed in high temperature, low temperature or high humidity environments, it is easy to have problems such as spraying sag, fly ash, and difficulty in receiving guns, and the adhesion to the water-based primer is poor, resulting in poor coating effect. ideal.
A composite paint film resin consisting of an aqueous hydroxyacrylate dispersion, an aqueous polycarbonate aliphatic anionic polyurethane dispersion with high glass transition temperature and an aqueous aliphatic anionic polyurethane dispersion with low glass transition temperature, and a composite paint film resin composed of an aqueous aliphatic anionic polyurethane dispersion with low glass transition temperature is used to provide specific preparations. The ratio and synergistic effect improves the solid content, thixotropy and adhesion of the paint film to form a high-gloss, flat and smooth coating.
The stable construction of water-based cover varnish is achieved in high temperature, low temperature or high humidity environments, which enhances the adhesion between layers with the water-based base paint, avoids sagging and fly ash, and improves the coating efficiency and appearance effect.
Smart Images

Figure BDA0004958859160000151 
Figure BDA0004958859160000161 
Figure BDA0004958859160000171
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of vehicle coatings, and in particular to a water-based topcoat varnish and a preparation method and application thereof. Background Art
[0002] Rail transit vehicles are a major means of transportation for the public. Most rail transit vehicles are manufactured using lightweight aluminum alloys instead of steel. With the change in the material of the carriages, the types and quality of coatings have also changed. Rail transit vehicles operate in various environments from C2 to C5, which determines that their coatings must take into account both anti-corrosion and decorative effects. The coating system of water-based basecoat + topcoat varnish has the advantages of low VOC content, fast drying, high hardness, impact resistance, strong adhesion, good appearance, excellent anti-corrosion performance, green and environmental protection, safe and convenient construction, and energy saving. It has become the mainstream direction of the development of the modern coatings industry.
[0003] When the "water-based basecoat + topcoat" system for rail transit vehicles is applied, the basecoat and topcoat are applied "wet on wet". During the conversion process of the water-based matching coating, due to the large construction area of the rail transit vehicle body painting, when the construction environment temperature is too high, too low or the humidity is high, spray sag, fly ash, and difficulty in connecting the gun are prone to occur. Therefore, the existing water-based topcoat must be applied under constant temperature and humidity conditions. In order to solve the problem of harsh basecoat construction conditions, it is urgent to find a water-based topcoat that can be applied in high temperature, low temperature or high humidity environments. At the same time, the paint film has excellent anti-sag, anti-prickly heat, anti-orange peel, anti-dark bubble and other characteristics. When spraying over a large area, the transition of the paint film joint is smooth, the surface is flat and smooth, and the interlayer adhesion of the "wet spray wet" coating with the water-based basecoat in the previous process is excellent, so as to meet the actual needs of the water-based topcoat in the application of rail transit vehicle painting. Summary of the invention
[0004] In view of the above problems, the present invention provides a water-based topcoat varnish and a preparation method and application thereof. Through the synergistic effect of various raw material components, it can be constructed on a large area under high temperature, low temperature or high humidity environment, cooperates well with the "wet spray wet" coating of water-based base paint, and has excellent comprehensive performance.
[0005] In order to solve the above technical problems, the technical solution provided by the present invention is:
[0006] In a first aspect, the present invention provides a water-based topcoat varnish, comprising a component A and a component B in a mass ratio of 6:1 to 2:1; wherein:
[0007] The component A comprises the following raw material components in percentage by mass: 40% to 50% of aqueous hydroxyl-containing acrylate dispersion, 10% to 25% of aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50°C, 0 to 25% of aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5°C, 0.2% to 1% of surfactant, 0.2% to 1% of defoaming agent, 0.2% to 1% of substrate wetting agent, 0.1% to 1% of leveling agent, 0.1% to 1% of aqueous ultraviolet absorber, 3% to 6% of first cosolvent, 1% to 3% of neutralizer, 0.2% to 0.5% of thickener and 5% to 15.5% of water;
[0008] The hydroxyl content of the aqueous hydroxyl-containing acrylate dispersion is 3% to 5%, and the solid content of the aqueous hydroxyl-containing acrylate dispersion is 40% to 50%;
[0009] The B component includes the following raw material components in percentage by mass: 70% to 80% of a curing agent and 20% to 30% of a second co-solvent; the curing agent is at least one of hexamethylene diisocyanate or a hydrophilic aliphatic polyisocyanate.
[0010] Compared with the prior art, the water-based topcoat varnish provided by the present invention comprises component A as a main paint component and component B as a curing component; component A is compounded with a water-based hydroxyl-containing acrylate dispersion and a water-based polycarbonate-containing aliphatic anionic polyurethane dispersion with a high glass transition temperature as a film-forming resin, and a water-based aliphatic anionic polyurethane dispersion with a low glass transition temperature is selectively added, and the characteristics of different types of water-based resins are brought into play to an optimal state through a specific ratio and the synergistic effect of each component, so that the finally obtained water-based topcoat varnish has a higher solid content, better thixotropy, good overlap when spraying over a large area (the overlapped edge portion when spraying multiple layers), excellent anti-sagging performance, good surface effect, high gloss, high distinctness and high fullness in the appearance of the paint film, and no drawbacks such as prickly heat, dark bubbles and orange peel texture, thereby solving the technical problem of poor fullness and appearance caused by low solid content in the construction of water-based varnish.
[0011] The paint film prepared by waterborne polyurethane dispersion is soft, has good thixotropic index and anti-sagging properties, and has a moderate drying speed. At the same time, it has good permeability, and different spraying techniques have little effect on the color effect of the topcoat varnish. The coating efficiency is high, and the bonding force with the upper and lower layers is also strong. When matched with waterborne basecoat, the coating is in a good state of "neither dry nor wet", which can ensure good interlayer adhesion and is not prone to "re-dissolution" (when matched with topcoat varnish wet spray, the cosolvent in the topcoat varnish will redissolve the basecoat). The flexibility of the molecular chain is the most important factor in determining the glass transition temperature (Tg, referred to as glass transition temperature) of the polymer. The better the flexibility of the main chain, the lower the glass transition temperature. The present invention finds through a large number of tests that an aqueous polyurethane dispersion with a low glass transition temperature can still maintain good flexibility in a low temperature environment and can improve the film-forming property under low temperature conditions; an aqueous polyurethane dispersion with a high glass transition temperature can improve the adaptability of the coating in a high temperature environment and enhance its high temperature resistance; and compounding aqueous polyurethane dispersions with different glass transition temperatures can adapt to and improve the paint film construction property under various complex conditions such as high temperature and low temperature, and can form a smooth and bright coating.
[0012] In addition, the water-based hydroxyl-containing acrylate dispersion is a secondary dispersion with the characteristics of high solid content (40% to 50%), high hydroxyl content (3% to 5%) and low volatile organic compound (VOC) content. The use of water-based hydroxyl-containing acrylate dispersion and polyisocyanate curing agent in the topcoat varnish has excellent reactivity and film-forming properties, which can make the topcoat varnish have good adhesion, durability, water resistance, solvent resistance and thermal stability, improve the flexibility and hardness of the coating film (above pencil hardness H), and make the coating have high gloss (60° gloss is 95%), high fullness, and high distinctness of image (DOI is above 90). Compared with low-hydroxyl acrylic resin, the hydroxyl value of water-based hydroxyl-containing acrylate dispersion is higher, and the number of hydroxyl groups in the film-forming resin will also increase accordingly, thereby improving the reactivity of the resin, so that the cross-linking speed and degree of cross-linking of the film-forming resin are significantly improved during curing. Due to the shortcomings of water-based hydroxyl-containing acrylate dispersions, such as fast drying, fast shrinkage of the paint film, many pits in the paint film, and obvious particles, the water-based topcoat varnish prepared by water-based hydroxyl-containing acrylate dispersions will have blue or white light on the side, which is difficult to adjust the color. Therefore, the use of water-based hydroxyl-containing acrylate dispersions alone as film-forming resins cannot meet the requirements of large-area spraying of rail transit vehicle bodies and rapid color adjustment of later repair paints. Compounding a specific proportion of water-based hydroxyl-containing acrylate dispersions in a hydroxyl-free water-based polyurethane dispersion can further enhance the adhesion of the paint film through chemical cross-linking of hydroxyl (-OH) and isocyanate (-NCO) curing agent; the synergistic effect of water-based polyurethane dispersions and water-based hydroxyl-containing acrylate dispersions can make up for the shortcomings of each single film-forming resin (single water-based polyurethane dispersions have poor self-thickening properties, low solid content, and poor water resistance, heat resistance and gloss of the paint film; single water-based acrylic resin emulsions are hot and viscous, cold and brittle, have poor flexibility, are not solvent-resistant, and are difficult to adjust the color).
[0013] The present invention obtains a water-based topcoat varnish with excellent comprehensive performance through the synergistic effect of each raw material component and a specific ratio content. The results of the embodiments show that the water-based topcoat varnish provided by the present invention can be applied on a large area under high temperature, low temperature or high humidity environment, and cooperates well with the "wet spray wet" coating of water-based base paint. Under the premise of not affecting the construction fluidity, it has excellent anti-sagging, color joint ability and interlayer adhesion, no fly ash, and at the same time has excellent mechanical properties and corrosion resistance, and has high practical value and promotion value.
[0014] It should be noted that the hydroxyl content of the aqueous hydroxyl-containing acrylate dispersion is calculated based on the calculated value of the solid resin.
[0015] Preferably, the viscosity of the aqueous hydroxyl-containing acrylate dispersion is 1000 mPa·s to 3000 mPa·s.
[0016] Preferably, the solid content of the aqueous hydroxyl-containing acrylate dispersion is 42% to 48%.
[0017] Preferably, the solid content of the aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50° C. and the aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature ≤ 5° C. are both 33% to 38%.
[0018] Preferably, the aqueous hydroxyl-containing acrylate dispersion is at least one of Bayhydrol A 2470 produced by Covestro or Bayhydrol A 2770 produced by Covestro.
[0019] Preferably, the aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion having a glass transition temperature of 40 to 50° C. is Bayhydol UH 2606 produced by Covestro.
[0020] Preferably, the aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5° C. is at least one of Bayhydrol UH 2648 / 1, Bayhydrol UH 2110, Bayhydrol UH 2621 or Bayhydrol UH 2952 / 1.
[0021] In the present invention, the aliphatic anionic polyurethane dispersion has the advantages of light color, high transparency, good compatibility, slightly slow drying speed, relatively soft paint film, moderate film volume shrinkage, strong corrosion resistance and strong interlayer adhesion, etc., which can minimize the interference with the color of the wet film state of the paint, have the fast color matching required by the repair paint, have excellent leveling, chemical resistance and weather resistance after film formation, and have high toughness and good elasticity. Among them, the water-based aliphatic anionic polyurethane dispersion with low glass transition temperature (especially Covestro Bayhydrol UH 2952 / 1) and the water-based polycarbonate-containing aliphatic anionic polyurethane dispersion with high glass transition temperature (Covestro Bayhydol UH 2606) can be attached to the body surface (or OEM product surface) without polishing, and have excellent adhesion and chemical resistance, which can not only meet the needs of large-area spraying of the whole vehicle body of rail transit vehicles, but also cooperate well with the "wet spray wet" coating of water-based base paint, and are also suitable for repairing paint under infrared baking lamps. The water-based hydroxyl-containing acrylate dispersion has a high content of hydroxyl groups in the molecules, fewer chemical bonds between molecules, and a more orderly arrangement between molecules, resulting in a lower viscosity; in addition, the higher the hydroxyl value, the better the reaction activity with the polyisocyanate curing agent, the greater the crosslinking density, and the better the adhesion and hardness after film formation. Adding a certain amount of high hydroxyl value resin to the film-forming resin and compounding it with the water-based polyurethane dispersion can not only improve the thixotropic index and anti-sagging properties of the coating, but also synergistically improve the flexibility and hardness of the coating, so that the coating has high gloss, high fullness, high distinctness, and excellent water resistance, solvent resistance and thermal stability.
[0022] Preferably, the surfactant is a gemini acetylenic diol surfactant.
[0023] Further preferably, the surfactant is at least one of Surfynol AD01, Surfynol 104BC or Surfynol 440.
[0024] More preferably, the surfactant is at least two of Surfynol AD01, Surfynol 104BC or Surfynol 440.
[0025] For example, the surfactant is Surfynol AD01, Surfynol 104BC and Surfynol 440 of Air Chemicals in a mass ratio of 2:1:1.
[0026] In the present invention, Surfynol AD01 is a Gemini acetylene glycol surfactant, HLB value (hydrophile-lipophile balance) = 4, has defoaming and wetting functions, can provide defoaming, dynamic wetting and help film formation effects; Surfynol 104BC is a Gemini tetramethyldecynediol nonionic surfactant, the dynamic surface tension of the wet film is slightly lower than the surface tension of the substrate, can well wet the substrate, form a continuous and stable paint film, has low water sensitivity, has wetting, leveling, defoaming, improves dispersibility, reduces surface tension and stabilizes consistency and viscosity and other functions; Surfynol 440 is a nonionic acetylene glycol ethoxylate, low dynamic tension, good compatibility, HLB value = 8, has Gemini wetting and low foaming effects, can reduce the dynamic and static surface tension of the system, and prevent the occurrence of shrinkage holes, pinholes and fish eyes.
[0027] Preferably, the defoaming agent is at least one of BYK-093, BYK-011 or TEGO-830.
[0028] Preferably, the substrate wetting agent is a polyether-modified silicone surfactant.
[0029] Further preferably, the substrate wetting agent is at least one of BYK-345, BYK-346, BYK-347, Tego-4100, Tego-280 or Surfynol 104BC.
[0030] The preferred substrate wetting agent of the present invention can effectively reduce the surface tension of the system, significantly improve the substrate wettability of the system, and at the same time has good recoatability without increasing the surface smoothness, and is suitable for all water-based systems without cosolvents.
[0031] Preferably, the leveling agent is at least one of BYK-378, BYK-381, BYK-333, BYK-331, Tego-4100 or Surfynol 104BC.
[0032] The paint molecules are constantly moving during the leveling process. As the viscosity of the paint gradually increases during the leveling process, the system molecules gradually form Bénard vortices, which leads to defects such as pinholes and sagging in the film-forming process. Among the preferred leveling agents of the present invention, BYK-378 is a polyether-modified dimethyl polysiloxane, which can significantly reduce the surface tension of the system, improve the surface smoothness, and thus improve the anti-scratch performance of the paint. It also has excellent substrate wettability and good anti-shrinkage effect, and has a good effect even at a low addition amount. It also has low foam stability, good compatibility, and is easy to recoat without causing oil spots; BYK-381 is an ionic polyacrylate solution type surface additive, which can improve the leveling and substrate wettability of the system and prevent surface defects (shrinkage and pinholes); Tego-4100 is a leveling agent with a twin structure, which has high activity and unstable foam. Even at extremely low concentrations, it can effectively reduce surface tension and improve wettability and leveling performance.
[0033] The dynamic surface tension of the wet film needs to be slightly lower than the surface tension of the substrate, so that the paint film can wet the substrate well and form a continuous and stable paint film. The preferred surfactants, substrate wetting agents and leveling agents of the present invention have low water sensitivity, which can effectively reduce the surface tension and achieve a balance between static and dynamic surface tensions. The special structure enables it to have wetting and defoaming effects, which can improve the dispersibility of the system, improve fluidity and leveling, control foam, and stabilize consistency and viscosity.
[0034] Preferably, the aqueous ultraviolet absorber is at least one of BASF Tinuvin 5151, Zhonghao Chemical UV-DL2, Everlight Chemical EVERSORB AQ1, Everlight Chemical EVERSORB AQ2 or Everlight Chemical EVERSORB AQ3.
[0035] In the present invention, Tinuvin 5151 light stabilizer is a synergistic mixture of hydrophilic 2-(2-hydroxyphenyl)-benzotriazole ultraviolet light absorber (UVA) and alkaline hindered amine radical scavenger (HALS), has excellent spectral coverage in the ultraviolet region, and the hydroxyl-containing ultraviolet light absorber can react with isocyanate and melamine crosslinking agents to reduce migration; UV-DL2 is a compound product of a high-efficiency ultraviolet light absorber and a light stabilizer, which can slow down the aging phenomena of the coating such as discoloration, gloss loss, cracking, detachment, etc. caused by light, improve the gloss retention rate, and thus improve the durability of the coating; EVERSORB AQ1, EVERSORBAQ2 and EVERSORB AQ3 are high-efficiency light stabilizers, which can inhibit the aging of the coating film and are suitable for transparent varnish.
[0036] Preferably, the first co-solvent includes at least three of propylene glycol methyl ether propionate, propylene glycol butyl ether, dipropylene glycol dimethyl ether, ethylene glycol butyl ether, dipropylene glycol methyl ether, dimethyl sulfoxide, N-methylpyrrolidone, dipropylene glycol butyl ether or diethylene glycol monobutyl ether.
[0037] Further preferably, based on the A component as 100%, the first co-solvent includes 1% to 2% of a first solvent, 0.75% to 1.5% of a second solvent and 1.25% to 2.5% of a third solvent; the first solvent includes at least one of propylene glycol methyl ether propionate (PMP), dipropylene glycol dimethyl ether (DMM) or propylene glycol butyl ether (PNB), the second solvent includes at least one of ethylene glycol butyl ether (BCS), dipropylene glycol methyl ether (DPM) or dimethyl sulfoxide (DMSO), and the third solvent includes at least one of N-methylpyrrolidone (NMP), diethylene glycol monobutyl ether (BDG) or dipropylene glycol butyl ether (DPNB).
[0038] More preferably, the first co-solvent comprises propylene glycol methyl ether propionate (PMP), dipropylene glycol methyl ether (DPM) and N-methylpyrrolidone (NMP) in a mass ratio of 1:1:1.
[0039] The present invention controls the boiling point (gradient boiling point) and solubility of the first cosolvent miscible with water (including the solubility of the solvent in water and the solubility of water in the solvent), which is beneficial to balancing the volatilization rate during the film-forming process, improving the solubility in water, and is more conducive to coating the paint film under high temperature or high humidity, with a moderate drying speed, no fly ash, no sagging, and no obvious traces of grabbing. As long as the ventilation conditions on site are good, normal coating can be performed. The specific first cosolvent can couple different phases, has a strong solubility for both polar and non-polar substances, interacts with the solution system in the water-based paint, causes it to produce a slight phase separation, helps to reduce the surface tension of the water-based system, enhances the fluidity of the paint, thereby adjusting its paint performance, increasing the viscosity of the water-based paint, changing the drying time of the paint, improving the wettability and coating effect of the paint, and improving the elasticity, wear resistance, water resistance, solvent resistance and mechanical strength of the paint film. The preferred first co-solvent can also be used as a film-forming aid. Its unique hydrophilic and lipophilic balance properties enable it to exert different film-forming effects on different resins, helping the coating to form a uniform and smooth coating. In particular, it can significantly reduce the surface tension of the system, assist in leveling, and prevent cracking and orange peel.
[0040] Preferably, the neutralizing agent is an 8 wt % to 12 wt % aqueous solution of dimethylethanolamine.
[0041] Preferably, the thickener is a polyurethane associative thickener.
[0042] Further preferably, the thickener is at least one of Hemmings RHEOLATE 299, BYK RHEOBYK-H 7625VF, Rohm and Haas RM5000 or Rohm and Haas RM-8W.
[0043] More preferably, the thickener is at least two of Hemmings RHEOLATE 299, BYK RHEOBYK-H 7625VF, Rohm and Haas RM5000 or Rohm and Haas RM-8W.
[0044] In the present invention, RHEOLATE 299, RHEOBYK-H 7625VF and RM5000 are the same type of polyurethane associative thickeners and are not affected by pH value; RHEOLATE 299 can provide efficient thickening in the medium and low shear rate range, RHEOBYK-H 7625VF can sharply increase the viscosity under low shear, and RM5000 can increase the viscosity in the high shear rate range, and the three play a complementary role; RM-8W is a low-odor, solvent-free, hydrophobically modified polyurethane nonionic associative thickener with excellent flow and leveling properties, uniform film-forming properties, glossiness and high thickening efficiency.
[0045] Preferably, the solid content of component A is 30% to 38%.
[0046] In the present invention, the solid content of component A refers to the mass ratio of all solid components in component A (including resin dispersion and pigment).
[0047] Preferably, based on 100% of the B component, the curing agent includes 25% to 30% of low-viscosity hydrophobic hexamethylene diisocyanate, 25% to 30% of high-viscosity hydrophilic hexamethylene diisocyanate and 18% to 22% of hydrophilic modified isophorone diisocyanate.
[0048] It should be noted that the hydrophilic modified isophorone diisocyanate in the present invention refers to a hydrophilic modified aliphatic polyisocyanate based on isophorone diisocyanate (IPDI).
[0049] Further preferably, the low-viscosity hydrophobic hexamethylene diisocyanate is at least one of Covestro Desmodur N3900, Covestro Desmodur N3600 or Wanhua WANNATE HT-600.
[0050] Further preferably, the high-viscosity hydrophilic hexamethylene diisocyanate is at least one of Bayhydrol XP2655, Bayhydur XP 2547, Bayhydur XP 2487 / 1, Bayhydur 304 or Bayhydur 305.
[0051] Preferably, the solid content of the hydrophilic aliphatic polyisocyanate is 60% to 70%.
[0052] Preferably, the -NCO content of the hydrophilic aliphatic polyisocyanate is 8.5% to 12%.
[0053] Further preferably, the hydrophilic aliphatic polyisocyanate is at least one of Covestro Bayhydur 401-70, Covestro Bayhydur 401-60 or Evonik Vestanat T1890E.
[0054] The present invention can further enhance the curing effect and improve the construction fluidity, viscosity and glossiness of the coating by limiting the type of curing agent.
[0055] Preferably, the second co-solvent is at least one of propylene glycol methyl ether acetate (PMA), propylene glycol methyl ether acrylate (PMP), propylene carbonate (PC), propylene glycol diacetate (PGDA), ethylene glycol butyl ether acetate (BGA), dibasic acid ester (DBE) or dipropylene glycol dimethyl ether (DMM).
[0056] In the present invention, a certain amount of the second cosolvent is added to the curing component, which can not only improve the compatibility of the curing agent with the aqueous hydroxyl-containing acrylate dispersion, but also prolong the open time of the paint film, which is beneficial to leveling. The specific second co-solvents are all environmentally friendly solvents with the following characteristics: (1) they contain multiple functional groups and have strong solubility for both polar and non-polar substances, which can improve the strength of the coating film; (2) they have low surface tension, strong solvent power, low viscosity and good volatility, which can provide good solubility and fluidity, ensure uniform coating and easy construction, and at the same time improve the adhesion and durability of the coating, adjust the volatilization rate of the entire system, adjust the drying speed of the paint film, reduce pinholes and fish eyes, and increase gloss, wetting, leveling and re-leveling properties; (3) propylene carbonate has good film-forming properties and strong carbon dioxide absorption capacity. When used with a hydrophilic isocyanate curing agent, the effect is excellent and can improve prickly heat and reduce bubbles; (4) The use of multiple second co-solvents can complement each other to achieve a better overall effect. In addition, by compounding second co-solvents with different boiling points (gradient boiling points), it is beneficial to balance the volatilization rate during the film-forming process and improve the solubility in water. For example, the synergy of propylene glycol methyl ether acetate (PMA), propylene glycol methyl ether propionate (PMP) and propylene carbonate (PC) can not only improve the strength of the coating film, but also facilitate the stable storage of the coating. It can also absorb carbon dioxide during the coating and film-forming process, and is extremely effective in diluting water-based isocyanate curing agents.
[0057] Preferably, the molar ratio of -NCO in the B component to -OH in the A component is 1.3:1 to 1.7:1, more preferably 1.4:1 to 1.6:1, and more preferably 1.5:1.
[0058] The preferred molar ratio of -NCO to -OH in the present invention can not only satisfy the combined application of component A and component B, but also, after adding a specific activated diluent during subsequent use, the ratio of -NCO to -OH in the system is more conducive to the formation of a paint film.
[0059] In a second aspect, the present invention provides a method for preparing a water-based topcoat varnish, comprising the following steps:
[0060] S1, weighing each raw material according to the designed ratio, adding an aqueous hydroxyl-containing acrylate dispersion, an aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50°C, and an aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5°C into water, mixing evenly, adding a surfactant, a defoamer, a substrate wetting agent, a leveling agent, an aqueous ultraviolet absorber and a first cosolvent, mixing evenly, and then adding a neutralizer and a thickener in sequence, mixing evenly, to obtain component A;
[0061] S2, adding the second co-solvent into the curing agent, mixing evenly, to obtain component B.
[0062] It should be noted that there is no order of precedence for steps S1 and S2.
[0063] The preparation method of the water-based finishing varnish provided by the invention does not require special treatment of raw materials and is simple and easy to implement.
[0064] For example, the preparation method of component A comprises the following steps:
[0065] Weigh the raw materials according to the designed ratio, add the aqueous hydroxyl-containing acrylate dispersion, the aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50°C, and the aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5°C into a clean container, add water at 600 rpm to 800 rpm, and stir for 4 to 6 minutes; then add the surfactant, defoamer, substrate wetting agent, leveling agent, aqueous ultraviolet absorber and the first cosolvent in sequence, and continue to stir at 600 rpm to 800 rpm for 10 to 15 minutes; then add the neutralizer to adjust the pH of the system to 8 to 8.5; finally add the thickener, mix well, and obtain component A.
[0066] In a third aspect, the present invention provides the use of the above-mentioned water-based topcoat varnish in automotive coatings.
[0067] Preferably, the vehicle coating is a coating for rail transit vehicles.
[0068] In a fourth aspect, the present invention provides a method for using the above-mentioned water-based topcoat varnish, comprising the following steps:
[0069] Mix component A and component B evenly, add an activated diluent, mix evenly to obtain a construction coating, and evenly apply it on the water-based base paint;
[0070] The activated diluent comprises an aqueous hydroxyl-containing acrylate dispersion, an aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50° C., an aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5° C., a water-based synthetic sheet silicate solution, a water-based modified urea solution, a first cosolvent, a stabilizer, a defoamer, a leveling agent and water.
[0071] In the method for using the water-based topcoat varnish, a unique activated diluent is used to dilute the water-based topcoat varnish (component A + component B), which has the following beneficial effects: (1) improving the system's tolerance to high levels of surfactants or extreme pH values; (2) preventing the paint from sagging or miscibility during "wet-on-wet" construction; and (3) accelerating the formation of the structure after construction during large-area spraying construction, thereby improving the adhesion of vertical surfaces (improving the interlayer adhesion between the water-based basecoat and the topcoat varnish) and preventing "re-dissolution".
[0072] Preferably, the activated diluent comprises the following raw material components in mass percentage: 8% to 11.5% of aqueous hydroxyl-containing acrylate dispersion, 3% to 4.5% of aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50°C, 3% to 4.5% of aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature ≤ 5°C, 25% to 33.5% of water-based synthetic sheet silicate solution, 0.5% to 0.7% of water-based modified urea solution, 7.5% to 8.5% of a first cosolvent, 7.5% to 8.5% of a stabilizer, 0.5% to 0.7% of a defoamer, 0.5% to 0.7% of a leveling agent and 27% to 42% of water, and the sum of each component is 100%.
[0073] Preferably, the mass ratio of the component A to the activated diluent is 100:(20-30).
[0074] The present invention adopts the above mass ratio to ensure the solid content of the construction coating. The specific amount of the activated diluent can be adjusted according to the ambient temperature and humidity and whether the construction spraying sags. Generally, the higher the temperature or humidity, the more the activated diluent is added; the more serious the sag phenomenon, the more the activated diluent is added.
[0075] Preferably, the hydroxyl content of the aqueous hydroxyl-containing acrylate dispersion is 3% to 5%.
[0076] Preferably, the viscosity of the aqueous hydroxyl-containing acrylate dispersion is 1000 mPa·s to 3000 mPa·s.
[0077] Preferably, the solid content of the aqueous hydroxyl-containing acrylate dispersion is 42% to 48%.
[0078] Preferably, the solid content of the aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50° C. and the aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature ≤ 5° C. are both 33% to 38%.
[0079] Preferably, the aqueous hydroxyl-containing acrylate dispersion is at least one of Bayhydrol A 2470 produced by Covestro or Bayhydrol A 2770 produced by Covestro.
[0080] Preferably, the aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion having a glass transition temperature of 40 to 50° C. is Bayhydol UH 2606 produced by Covestro.
[0081] Preferably, the aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5° C. is at least one of Bayhydrol UH 2648 / 1, Bayhydrol UH 2110, Bayhydrol UH 2621 or Bayhydrol UH 2952 / 1.
[0082] Preferably, the water-based synthetic sheet silicate solution comprises the following raw material components in percentage by mass: 1.5% to 2.5% of organic modified synthetic layer silicate, 1.5% to 2.5% of emulsifying dispersant and 95% to 97% of water, and the sum of the components is 100%.
[0083] More preferably, the organic-modified synthetic layered silicate is at least one of BYK Laponite-RD or BYK Laponite-RDS.
[0084] Laponite-RD and Laponite-RDS are synthetic sheet silicates that are insoluble in water but can hydrate and swell in water to form a colorless and transparent colloid. When the concentration in water is above 2%, a colloid with improved thixotropy can be formed, which plays an activation and regulating role in anti-sagging. The present invention utilizes the synergistic effect of the compounding of LAPONITE and polymer to improve the tolerance of the system to high content of surfactants, electrolytes or extreme pH values.
[0085] Further preferably, the emulsifying dispersant is at least one of polyethylene glycol and polypropylene glycol. If the emulsifying dispersant includes polyethylene glycol and polypropylene glycol, the mass ratio of polyethylene glycol to polypropylene glycol may be 1:1.
[0086] More preferably, the emulsifying dispersant is at least one of PEG-1000, PEG-1500, PPG-200, PPG-400 or PPG-600.
[0087] Preferably, the method for preparing the water-based synthetic sheet silicate solution comprises the following steps:
[0088] The emulsifying dispersant is added into water and mixed evenly, and then the organic modified synthetic layered silicate is added and mixed evenly to obtain a water-based synthetic sheet silicate solution.
[0089] For example, under stirring at 400 rpm to 600 rpm, an emulsifying dispersant is added to water, the rotation speed is adjusted to 1000 rpm to 1500 rpm, and the organic modified synthetic layered silicate is slowly added, and stirring is continued until the solution is clear and no dissolved particles are seen, thereby obtaining a water-based synthetic sheet silicate solution.
[0090] Preferably, the water-based modified urea solution is at least one of BYK RHEOBYK-7420CA, BYK RHEOBYK-7420ET or BYK RHEOBYK-7420ES.
[0091] In the present invention, the water-based modified urea solution is a liquid rheological agent, and a specific amount of the water-based modified urea solution can produce a strong thixotropic effect, thereby improving the anti-settling and anti-sagging properties of the system.
[0092] Preferably, the first co-solvent includes at least three of propylene glycol methyl ether propionate, propylene glycol butyl ether, dipropylene glycol dimethyl ether, ethylene glycol butyl ether, dipropylene glycol methyl ether, dimethyl sulfoxide, N-methylpyrrolidone, dipropylene glycol butyl ether or diethylene glycol monobutyl ether.
[0093] Further preferably, based on the A component as 100%, the first co-solvent includes 1% to 2% of a first solvent, 0.75% to 1.5% of a second solvent and 1.25% to 2.5% of a third solvent; the first solvent includes at least one of propylene glycol methyl ether propionate (PMP), dipropylene glycol dimethyl ether (DMM) or propylene glycol butyl ether (PNB), the second solvent includes at least one of ethylene glycol butyl ether (BCS), dipropylene glycol methyl ether (DPM) or dimethyl sulfoxide (DMSO), and the third solvent includes at least one of N-methylpyrrolidone (NMP), diethylene glycol monobutyl ether (BDG) or dipropylene glycol butyl ether (DPNB).
[0094] Preferably, the stabilizer is at least one of propylene glycol methyl ether acetate (PGMEA) or propylene glycol methyl ether propionate (PMP).
[0095] In the present invention, the preferred stabilizer can provide good solubility and fluidity, ensure uniform coating and easy construction, and improve the adhesion and durability of the coating.
[0096] Preferably, the defoaming agent is at least one of BYK-093, BYK-011 or TEGO-830.
[0097] Preferably, the leveling agent is at least one of BYK-378, BYK-381, BYK-333, BYK-331, Tego-4100 or Surfynol 104BC.
[0098] For example, the preparation method of the activated diluent comprises the following steps:
[0099] Weigh the raw materials according to the designed ratio, add an aqueous hydroxyl-containing acrylate dispersion, an aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50°C, an aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5°C, a defoamer, a leveling agent, a first cosolvent, a stabilizer, a water-based synthetic sheet silicate solution and a water-based modified urea solution into water at 400 rpm to 600 rpm, and continue stirring at 600 rpm to 800 rpm for 8 min to 12 min to obtain an activated diluent.
[0100] The corresponding film-forming resin in component A is added to the activated diluent of the present invention, which increases the solid content of the construction and the hydroxyl content, further promotes the reaction activity of the film-forming resin and the isocyanate curing agent, thereby enhancing the adhesion, and improving the gloss, distinctness and fullness of the paint film; through the synergistic effect of compounding the aqueous hydroxyl-containing acrylate dispersion and the aqueous polyurethane dispersion with different glass transition temperatures, the tolerance of the system to the ultimate film thickness of the topcoat varnish is improved, and an ideal paint film surface state can be formed after accelerated construction, which is particularly suitable for large-area construction spraying of rail transit vehicle bodies, and can be smoothly constructed under high temperature, low temperature or high humidity environments. The water-based modified urea solution is a liquid rheological agent, which can produce a strong thixotropic effect and can improve the anti-settling and anti-sagging properties of water-based and high-polarity systems. In addition, the stabilizer is a high-grade industrial solvent with excellent performance. It has strong solubility and fluidity for both polar and non-polar substances, which can ensure uniform coating and easy construction, further improve the adhesion and durability of the coating, and at the same time improve the solubility of the water-based synthetic sheet silicate solution, ensuring that the coating can be stored for a long time without flocculation and agglomeration. During construction, by adding an activated diluent, the interlayer adhesion can be greatly improved and the rheological properties can be accurately adjusted, thereby improving the interlayer adhesion between the topcoat varnish and the water-based basecoat, and further preventing the topcoat varnish from being "re-dissolved" by the basecoat and losing its gloss.
[0101] The water-based synthetic sheet silicate solution and the water-based modified urea solution can form a synergistic effect, increase the low shear viscosity of the coating, prevent the coating from sagging or mixing during "wet-on-wet" construction, improve the construction and storage stability of the coating, and effectively prevent the sedimentation and dehydration shrinkage of solid matter in the water-based coating system, thereby accelerating the formation of the structure after construction. The present invention has found through a large number of experiments that when the rheological additive water-based synthetic sheet silicate solution and the surfactant water-based modified urea solution are compounded, if the rheological additive is used in excessive amounts, it will cause the activation dilution to be unable to be stored for a long time (caking and flocculation will occur after long storage), and it will also cause the water resistance of the water-based topcoat varnish to deteriorate; if the surfactant is used in excessive amounts, it will cause the paint film to have defects such as shrinkage cavities, prickly heat, and orange peel. Therefore, the rheological additive is compounded with the surface additive, stabilizer and other additives and part of the film-forming resin in a specific ratio, which further improves the storage stability and water resistance of the coating, and makes the appearance of the paint film reach the best state. DETAILED DESCRIPTION
[0102] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0103] The water used in the embodiments of the present invention is deionized water.
[0104] The test instrument used in the present invention comprises:
[0105] Grid marker, Guangzhou Biaogeda;
[0106] Pencil hardness tester, impact instrument, bending tester, cupping tester, distinctness of image tester, BYK, Germany;
[0107] MA85 multi-angle wind photometer, X-Rite, USA;
[0108] ISO No. 6 cup, Tu-4# cup, solvent resistance wiper, pH meter, film thickness meter, Shanghai Modern Environmental Engineering Technology Co., Ltd.;
[0109] Salt spray resistance test equipment, artificial weathering resistance (QUA / SPARY), Q-Lab, USA.
[0110] In order to better illustrate the present invention, further examples are given below.
[0111] Example 1
[0112] This embodiment provides a water-based topcoat varnish, which is composed of component A and component B in a mass ratio of 4:1.
[0113] Component A is composed of the following raw material components in percentage by mass: 50% aqueous hydroxyl acrylate dispersion, 18% aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50°C (denoted as PUD with Tg=40-50), 13% aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5°C (denoted as PUD with Tg≤5), 0.6% surfactant, 0.6% defoaming agent, 0.6% substrate wetting agent, 0.6% leveling agent, 0.6% aqueous ultraviolet absorber, 4% first cosolvent, 2% neutralizer, 0.3% thickener and 9.7% water.
[0114] Component B is composed of the following raw material components in percentage by mass: 75% of curing agent (28% of low viscosity hydrophobic hexamethylene diisocyanate, 27% of high viscosity hydrophilic hexamethylene diisocyanate and 20% of hydrophilic modified isophorone diisocyanate) and 25% of the second cosolvent.
[0115] The specific components of the above raw materials are shown in Table 1. After calculation, the solid content of component A is 34.6%.
[0116] The preparation method of the above-mentioned water-based topcoat varnish comprises the following steps:
[0117] S1, weigh the raw materials according to the designed ratio, add the aqueous hydroxyl-containing acrylate dispersion, the aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40-50°C, and the aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5°C into a clean container, add water at 700rpm, and stir for 5min; then add the surfactant, defoamer, substrate wetting agent, leveling agent, aqueous ultraviolet absorber and the first cosolvent in sequence, and continue to stir at 700rpm for 13min; then add the neutralizer to adjust the pH of the system to 8.5; finally add the thickener, mix well, and obtain component A.
[0118] S2, adding the second co-solvent into the curing agent, mixing evenly, to obtain component B.
[0119] Example 2
[0120] This embodiment provides a water-based topcoat varnish, which is composed of component A and component B in a mass ratio of 4.5:1.
[0121] Component A is composed of the following raw material components in percentage by mass: 45% aqueous hydroxyl-containing acrylate dispersion, 10% aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50°C, 20% aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5°C, 0.8% surfactant, 0.8% defoaming agent, 0.8% substrate wetting agent, 0.8% leveling agent, 0.8% aqueous ultraviolet absorber, 5% first cosolvent, 2% neutralizer, 0.4% thickener and 13.6% water.
[0122] Component B is composed of the following raw material components in percentage by mass: 73% of curing agent (30% of low viscosity hydrophobic hexamethylene diisocyanate, 25% of high viscosity hydrophilic hexamethylene diisocyanate and 18% of hydrophilic modified isophorone diisocyanate) and 27% of the second cosolvent.
[0123] The specific components of the above raw materials are shown in Table 1. After calculation, the solid content of component A is 32.4%.
[0124] The preparation method of the above-mentioned water-based topcoat varnish comprises the following steps:
[0125] S1, weigh the raw materials according to the designed ratio, add the aqueous hydroxyl-containing acrylate dispersion, the aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40-50°C, and the aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5°C into a clean container, add water at 800rpm, and stir for 4min; then add the surfactant, defoamer, substrate wetting agent, leveling agent, aqueous ultraviolet absorber and the first cosolvent in sequence, and continue to stir at 800rpm for 10min; then add the neutralizer to adjust the pH of the system to 8.5; finally add the thickener, mix well, and obtain component A.
[0126] S2 is the same as in Example 1 and will not be described in detail.
[0127] Example 3
[0128] This embodiment provides a water-based topcoat varnish, which is composed of component A and component B in a mass ratio of 4.8:1.
[0129] Component A is composed of the following raw material components in percentage by mass: 40% aqueous hydroxyl-containing acrylate dispersion, 25% aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50°C, 25% aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5°C, 0.2% surfactant, 0.2% defoamer, 0.2% substrate wetting agent, 0.1% leveling agent, 0.1% aqueous ultraviolet absorber, 3% first cosolvent, 1% neutralizer, 0.2% thickener and 5% water.
[0130] Component B is composed of the following raw material components in percentage by mass: 80% of curing agent (28% of low viscosity hydrophobic hexamethylene diisocyanate, 30% of high viscosity hydrophilic hexamethylene diisocyanate and 22% of hydrophilic modified isophorone diisocyanate) and 20% of the second cosolvent.
[0131] The specific components of the above raw materials are shown in Table 1. After calculation, the solid content of component A is 35.9%.
[0132] The preparation method of the above-mentioned water-based topcoat varnish comprises the following steps:
[0133] S1, weigh the raw materials according to the designed ratio, add the aqueous hydroxyl-containing acrylate dispersion, the aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40-50°C, and the aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5°C into a clean container, add water at 600rpm, and stir for 6min; then add the surfactant, defoamer, substrate wetting agent, leveling agent, aqueous ultraviolet absorber and the first cosolvent in sequence, and continue to stir at 600rpm for 15min; then add the neutralizer to adjust the pH of the system to 8; finally add the thickener, mix well, and obtain component A.
[0134] S2 is the same as in Example 1 and will not be described in detail.
[0135] Example 4
[0136] This embodiment provides a water-based topcoat varnish, which is composed of component A and component B in a mass ratio of 5.4:1.
[0137] Component A is composed of the following raw material components in percentage by mass: 45% aqueous hydroxyl-containing acrylate dispersion, 25% aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50° C., 1% surfactant, 1% defoamer, 1% substrate wetting agent, 1% leveling agent, 1% aqueous ultraviolet absorber, 6% first cosolvent, 3% neutralizer, 0.5% thickener and 15.5% water.
[0138] Component B is composed of the following raw material components in percentage by mass: 75% of curing agent (55% of high viscosity hydrophobic hexamethylene diisocyanate and 20% of hydrophilic modified isophorone diisocyanate) and 25% of the second co-solvent.
[0139] The specific components of the above raw materials are shown in Table 1. After calculation, the solid content of component A is 31.1%.
[0140] The preparation method of the above-mentioned water-based topcoat varnish is the same as that of Example 1 and will not be repeated here.
[0141] Example 5
[0142] This embodiment provides a water-based topcoat varnish, which is composed of component A and component B in a mass ratio of 5.8:1.
[0143] Component A is composed of the following raw material components in percentage by mass: 45% aqueous hydroxyl-containing acrylate dispersion, 23% aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50°C, 5% aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5°C, 0.7% surfactant, 0.7% defoaming agent, 0.7% substrate wetting agent, 0.7% leveling agent, 0.7% aqueous ultraviolet absorber, 5% first cosolvent, 3% neutralizer, 0.4% thickener and 15.1% water.
[0144] Component B is composed of the following raw material components in percentage by mass: 75% of curing agent (75% of high viscosity hydrophilic hexamethylene diisocyanate) and 25% of the second co-solvent.
[0145] The specific components of the above raw materials are shown in Table 1. After calculation, the solid content of component A is 31.5%.
[0146] The preparation method of the above-mentioned water-based topcoat varnish is the same as that of Example 1 and will not be repeated here.
[0147] Example 6
[0148] This embodiment provides a water-based topcoat varnish, which is composed of component A and component B in a mass ratio of 2:1. The raw materials and contents of component A are the same as those in Example 1 and are not described in detail. Component B replaces all the curing agents in Example 1 with hydrophilic modified isophorone diisocyanate (Covestro Bayhydur 401-60) of equal mass percentage, and the remaining components and corresponding contents are the same as those in Example 1 and are not described in detail.
[0149] The preparation method of the above-mentioned water-based topcoat varnish is the same as that of Example 1 and will not be repeated here.
[0150] Table 1 Specific raw material components of water-based finish varnishes in Examples 1 to 5
[0151]
[0152]
[0153]
[0154] Comparative Example 1
[0155] This comparative example provides a water-based topcoat varnish, which is similar to Example 1, except that Covestro Bayhydrol A 2470 is replaced with Covestro Bayhydol UH 2606 of equal quality (i.e., the water-based resin does not contain a water-based hydroxyl-containing acrylate dispersion). The remaining components are the same as those in Example 1 and are not described in detail.
[0156] Comparative Example 2
[0157] This comparative example provides a water-based topcoat varnish, which is similar to Example 1, except that Covestro Bayhydol UH 2606 is replaced with Covestro Bayhydrol A 2470 of equal quality (i.e., the water-based resin does not contain a water-based polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50° C.). The remaining components are the same as those in Example 1 and are not described in detail.
[0158] Comparative Example 3
[0159] This comparative example provides a water-based topcoat varnish, which is similar to Example 1, except that Covestro Bayhydol UH 2606 and Bayhydrol UH 2952 / 1 are replaced with Covestro Bayhydrol A 2470 of equal quality (i.e., the water-based resin contains only water-based hydroxyl-containing acrylate dispersion). The remaining components are the same as those in Example 1 and are not described in detail.
[0160] Comparative Example 4
[0161] This comparative example provides a water-based topcoat varnish, which is similar to Example 1, except that Covestro Bayhydrol A 2470 and Bayhydrol UH 2952 / 1 are replaced by Covestro Bayhydol UH 2606 of equal quality (i.e., the water-based resin contains only a water-based polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50° C.). The remaining components are the same as those in Example 1 and are not described in detail.
[0162] Comparative Example 5
[0163] This comparative example provides a water-based topcoat varnish, which is similar to Example 1, except that Covestro Bayhydol UH 2606 and Bayhydrol A 2470 are replaced by Covestro Bayhydrol UH 2952 / 1 of equal quality (i.e., the water-based resin contains only a water-based polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5°C). The remaining components are the same as those in Example 1 and are not described in detail.
[0164] Comparative Example 6
[0165] This comparative example provides a water-based topcoat varnish, which is similar to Example 1, except that the water-based resin (Covestro Bayhydol UH 2606, Bayhydrol A 2470 and Bayhydrol UH 2952 / 1) is replaced with Uacryl 4219 (acrylic emulsion). The remaining components are the same as those in Example 1 and are not described in detail.
[0166] Comparative Example 7
[0167] This comparative example provides a water-based topcoat varnish, which is similar to Example 1, except that Covestro Bayhydol UH 2606 and Bayhydrol UH 2952 / 1 are replaced by allnex of equal quality. 6803 (water-based acrylic resin emulsion). The remaining components are the same as those in Example 1 and will not be described in detail.
[0168] Application Example 1
[0169] This application embodiment provides a method for using a water-based topcoat varnish, comprising the following steps:
[0170] The components A and B of Example 1 were mixed evenly, and an activated diluent was added and mixed evenly to obtain a construction coating. The mass ratio of the component A to the activated diluent was 100:25.
[0171] The activated diluent is composed of the following raw material components in percentage by mass: 10% aqueous hydroxyl-containing acrylate dispersion, 4% aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50°C, 4% aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5°C, 29% water-based synthetic sheet silicate solution, 0.6% water-based modified urea solution, 8% first cosolvent, 8% stabilizer, 0.6% defoamer, 0.6% leveling agent and 35.2% water.
[0172] The water-based synthetic sheet silicate solution is composed of the following raw materials in percentage by mass: 2% of organic modified synthetic layer silicate, 2% of emulsifying dispersant and 96% of water.
[0173] It should be noted that the aqueous hydroxyl-containing acrylate dispersion, the aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50° C., the aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5° C., the first cosolvent, the defoamer and the leveling agent in the activated diluent are the same as the corresponding raw material components in component A of Example 1. The specific components of the remaining raw materials are shown in Table 2.
[0174] Application Example 2
[0175] This application embodiment provides a method for using a water-based topcoat varnish, comprising the following steps:
[0176] The components A and B of Example 2 were mixed evenly, and an activated diluent was added and mixed evenly to obtain a construction coating. The mass ratio of the component A to the activated diluent was 100:20.
[0177] The activated diluent is composed of the following raw material components in percentage by mass: 11.5% aqueous hydroxyl-containing acrylate dispersion, 4.5% aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50°C, 4.5% aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5°C, 33.5% water-based synthetic sheet silicate solution, 0.7% water-based modified urea solution, 8.4% first cosolvent, 8.5% stabilizer, 0.7% defoamer, 0.7% leveling agent and 27% water.
[0178] The water-based synthetic sheet silicate solution is composed of the following raw materials in percentage by mass: 1.5% of organic modified synthetic layer silicate, 1.5% of emulsifying dispersant and 97% of water.
[0179] It should be noted that the aqueous hydroxyl-containing acrylate dispersion, the aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50° C., the aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5° C., the first cosolvent, the defoamer and the leveling agent in the activated diluent are the same as the corresponding raw material components in component A of Example 2. The specific components of the remaining raw materials are shown in Table 2.
[0180] Application Example 3
[0181] This application embodiment provides a method for using a water-based topcoat varnish, comprising the following steps:
[0182] The components A and B of Example 3 were mixed evenly, and an activated diluent was added and mixed evenly to obtain a construction coating. The mass ratio of the component A to the activated diluent was 100:30.
[0183] The activated diluent is composed of the following raw material components in percentage by mass: 8.1% aqueous hydroxyl-containing acrylate dispersion, 3.1% aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50°C, 3.1% aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5°C, 27% water-based synthetic sheet silicate solution, 0.5% water-based modified urea solution, 7.6% first cosolvent, 7.6% stabilizer, 0.5% defoamer, 0.5% leveling agent and 42% water.
[0184] The water-based synthetic sheet silicate solution is composed of the following raw materials in percentage by mass: 2.5% of organic modified synthetic layer silicate, 2.5% of emulsifying dispersant and 95% of water.
[0185] It should be noted that the aqueous hydroxyl-containing acrylate dispersion, the aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50° C., the aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5° C., the first cosolvent, the defoamer and the leveling agent in the activated diluent are the same as the corresponding raw material components in component A of Example 3. The specific components of the remaining raw materials are shown in Table 2.
[0186] Application Example 4
[0187] This application embodiment provides a method for using a water-based topcoat varnish, comprising the following steps:
[0188] The components A and B of Example 4 were mixed evenly, and an activated diluent was added and mixed evenly to obtain a construction coating. The mass ratio of the component A to the activated diluent was 100:25.
[0189] The raw material ratio of the activated diluent and the raw material ratio of the water-based synthetic sheet silicate solution are the same as those in Application Example 1; the aqueous hydroxyl-containing acrylate dispersion, the aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50°C, the aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5°C, the first cosolvent, the defoamer and the leveling agent in the activated diluent are the same as the corresponding raw material components in component A of Example 4. The specific components of the remaining raw materials are shown in Table 2.
[0190] Application Example 5
[0191] This application embodiment provides a method for using a water-based topcoat varnish, comprising the following steps:
[0192] The components A and B of Example 5 were mixed evenly, and the activated diluent was added and mixed evenly to obtain a construction coating. The mass ratio of the component A to the activated diluent was 100:25.
[0193] The raw material ratio of the activated diluent and the raw material ratio of the water-based synthetic sheet silicate solution are the same as those in Application Example 1; the aqueous hydroxyl-containing acrylate dispersion, aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50°C, aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5°C, the first cosolvent, defoamer and leveling agent in the activated diluent are the same as the corresponding raw material components in component A of Example 5. The specific components of the remaining raw materials are shown in Table 2.
[0194] Application Example 6
[0195] This application embodiment provides a method for using a water-based topcoat varnish, comprising the following steps:
[0196] The components A and B of Example 6 were mixed evenly, and the activated diluent was added and mixed evenly to obtain a construction coating. The mass ratio of the component A to the activated diluent was 100:25.
[0197] The raw material ratio and components of the activated diluent are the same as those in Application Example 1 and will not be described in detail.
[0198] Table 2 Specific raw material components of the activated diluent in Application Examples 1 to 5
[0199]
[0200] Application Comparative Examples 1 to 7
[0201] Comparative Examples 1 to 7 provide a method for using a water-based topcoat varnish, respectively, comprising the following steps:
[0202] Components A and B of Comparative Examples 1 to 7 were mixed evenly, and activated diluent was added and mixed evenly to obtain 7 groups of construction coatings. The mass ratio of component A to activated diluent was 100:25. The raw material components and proportions of the activated diluent were the same as those of Application Example 1, and will not be described in detail.
[0203] Application Comparative Example 8
[0204] This application comparative example provides a method for using a water-based topcoat varnish, comprising the following steps:
[0205] The components A and B of Example 1 were mixed evenly, and water was added and mixed evenly to obtain a construction coating. The mass ratio of the component A to water was 100:25.
[0206] Application Comparative Example 9
[0207] This comparative application example provides a method for using a water-based topcoat varnish, which is similar to Application Example 1, except that the water-based polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50° C. in the activated diluent is replaced with an equal amount of water-based hydroxyl-containing acrylate dispersion. The remaining conditions are the same as those in Application Example 1 and are not described in detail.
[0208] Application Comparative Example 10
[0209] This comparative application example provides a method for using a water-based topcoat varnish, which is similar to Application Example 1, except that the water-based modified urea solution in the activation diluent is replaced with an equal amount of water-based synthetic sheet silicate solution. The remaining conditions are the same as those in Application Example 1 and will not be described in detail.
[0210] Performance Testing
[0211] The performance tests were conducted on the construction coatings provided in Application Examples 1 to 6 and Application Comparative Examples 1 to 10.
[0212] (1) The tinplate was polished with 400-500 mesh sandpaper, and the surface oil was removed with ethanol, and then the construction coatings provided in application examples 1-6 and application comparative examples 1-10 were coated, such as: the construction coatings provided in application examples 1-2, 6 and application comparative examples 1-4 were coated at high temperature and high humidity (38°C, RH=85%), and the construction coatings provided in application examples 3-5 and application comparative examples 5-10 were coated at low temperature and high humidity (0°C, RH=85%); the film thickness was 20μm-30μm, and baked at 60°C for 2h. The paint film color and appearance, drying time, impact resistance, bending test and cupping test of the obtained test sample were tested respectively, and the test standards are shown in Table 3, and the test results are shown in Tables 4-5.
[0213] (2) On the cathode electrophoretic paint (CED, model EcoTa8500, purchased from Shanghai Jinlitai Chemical Co., Ltd.) steel plate, WB07-1 intermediate paint (purchased from Beijing Yulin Chemical Co., Ltd.) was coated with a film thickness of 40 μm to 60 μm and baked at 60°C for 2 h; then WB03-05 water-based base paint (purchased from Beijing Yulin Chemical Co., Ltd.) was coated on the WB07-1 intermediate paint with a film thickness of 20 μm to 30 μm, and allowed to stand at room temperature for about 30 min until the surface was dry (or baked at 60°C for 10 min). min); then apply the construction coatings provided in application examples 1 to 6 and application comparative examples 1 to 10, such as: apply the construction coatings provided in application examples 3 to 5 and application comparative examples 1 to 4 at high temperature and high humidity (38°C, RH=85%), and apply the construction coatings provided in application examples 1 to 2, 6 and application comparative examples 5 to 10 at low temperature and high humidity (0°C, RH=85%); spray 2 to 3 coats, flash dry for 5min to 10min each coat, and pre-bake at 60°C for 10min (the paint film is dry on the surface). The solvent wiping resistance, water resistance, gasoline resistance, acid resistance, acid resistance, alkali resistance and artificial weather accelerated aging resistance of the obtained test sample were tested respectively, and the test standards are shown in Table 3, and the test results are shown in Tables 4 to 5.
[0214] Table 3 Performance test standards and requirements of the construction coatings provided in the application examples and comparative examples
[0215]
[0216]
[0217] Table 4 Performance test results of the construction coating provided by the application example
[0218]
[0219]
[0220] In the table:
[0221] Thixotropic index: measured using NDJ-1 rotary viscometer; viscosity of component A is adjusted by the amount of thickener (ISO6 # ) is about 70s, and its low rotation (6r / min) viscosity and high rotation (60r / min) viscosity are measured. The calculation formula of thixotropic index is: thixotropic index (DI) = low rotation viscosity / high rotation viscosity.
[0222] Appearance effect evaluation: 0 is "excellent", 1 is "qualified", and the larger the number is, the worse it is. 0-smooth and delicate; 1-not delicate enough; 2-slight orange peel; 3-rough paint film with many pits; 4-obvious orange peel, paint film sagging, dark.
[0223] Construction performance: 0 is "excellent", 1 is "qualified", and the larger the number is, the worse it is. 0-the paint film is smooth and flat, without sagging; 1-slight orange peel; 2-slight sagging; 3-slight orange peel and slight sagging; 4-fly ash, particles, poor fluidity; 5-severe orange peel and severe sagging.
[0224] Cross-cut test: 0 means "excellent", 1 means "qualified", and the larger the number is, the worse it is. 0-The substrate is not polished, and the adhesion is excellent; the rest is based on the cross-cut test standard GB / T9286-1998 "Cross-cut test for paint and varnish film".
[0225] Table 5 Performance test results of the construction coating provided by the comparative example
[0226]
[0227]
[0228]
[0229] In summary, the water-based topcoat varnish provided by the present invention, component A selects water-based hydroxyl-containing acrylate dispersion and water-based polycarbonate-containing aliphatic anionic polyurethane dispersion with high glass transition temperature for compounding as film-forming resin, and selectively adds water-based aliphatic anionic polyurethane dispersion with low glass transition temperature, and through specific ratios and the synergistic effect of each component, the characteristics of different types of water-based resins are brought into play to the best state, so that the final water-based topcoat varnish has good thixotropy, and the paint film has excellent characteristics such as high gloss, high distinctness, high fullness and small orange grain, and no fly ash is produced when spraying over a large area, the gun is well mounted, and the thixotropy is improved, while balancing the flexibility and hardness of the cured film, which can effectively solve the problem of "wet spray wet" matching coating construction difficulties in the "water-based base paint + topcoat varnish" system, and can be constructed over a large area under high temperature, low temperature or high humidity. The present invention obtains a water-based topcoat varnish with excellent comprehensive performance through the synergistic effect of each raw material component and a specific ratio content, and has high practical value and promotion value.
[0230] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A water-based topcoat varnish, characterized in that: It is composed of component A and component B in a mass ratio of 6:1 to 2:1; wherein, The component A comprises the following raw material components in percentage by mass: 40% to 50% of aqueous hydroxyl-containing acrylate dispersion, 10% to 25% of aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50°C, 0 to 25% of aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5°C, 0.2% to 1% of surfactant, 0.2% to 1% of defoaming agent, 0.2% to 1% of substrate wetting agent, 0.1% to 1% of leveling agent, 0.1% to 1% of aqueous ultraviolet absorber, 3% to 6% of first cosolvent, 1% to 3% of neutralizer, 0.2% to 0.5% of thickener and 5% to 15.5% of water; The hydroxyl content of the aqueous hydroxyl-containing acrylate dispersion is 3% to 5%, and the solid content of the aqueous hydroxyl-containing acrylate dispersion is 40% to 50%; The B component includes the following raw material components in percentage by mass: 70% to 80% of a curing agent and 20% to 30% of a second co-solvent; the curing agent is at least one of hexamethylene diisocyanate or a hydrophilic aliphatic polyisocyanate.
2. The water-based finishing varnish according to claim 1, characterized in that: The viscosity of the aqueous hydroxyl-containing acrylate dispersion is 1000 mPa·s to 3000 mPa·s; The solid contents of the aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50° C. and the aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5° C. are both 33% to 38%.
3. The water-based finishing varnish according to claim 1, characterized in that: The aqueous hydroxyl-containing acrylate dispersion is at least one of Covestro Bayhydrol A 2470 and Covestro Bayhydrol A 2770; The aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion having a glass transition temperature of 40 to 50° C. is Bayhydol UH 2606 from Covestro; The aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5° C. is at least one of Bayhydrol UH2648 / 1, Bayhydrol UH 2110, Bayhydrol UH 2621 or Bayhydrol UH2952 / 1.
4. The water-based finishing varnish according to claim 1, characterized in that: Taking the B component as 100%, the curing agent comprises 25% to 30% of low-viscosity hydrophobic hexamethylene diisocyanate, 25% to 30% of high-viscosity hydrophilic hexamethylene diisocyanate and 18% to 22% of hydrophilic modified isophorone diisocyanate; wherein, The solid content of the hydrophilic aliphatic polyisocyanate is 60% to 70%, and the -NCO content of the hydrophilic aliphatic polyisocyanate is 8.5% to 12%.
5. The water-based finishing varnish according to claim 4, characterized in that: The low-viscosity hydrophobic hexamethylene diisocyanate is at least one of Covestro Desmodur N3900, Covestro Desmodur N3600 or Wanhua WANNATE HT-600; The high-viscosity hydrophilic hexamethylene diisocyanate is at least one of Covestro Bayhydrol XP 2655, Covestro Bayhydur XP 2547, Covestro Bayhydur XP 2487 / 1, Covestro Bayhydur 304 or Covestro Bayhydur 305; The hydrophilic aliphatic polyisocyanate is at least one of Covestro Bayhydur 401-70 and Covestro Bayhydur 401-60.
6. The water-based topcoat varnish according to any one of claims 1 to 5, characterized in that: The first cosolvent comprises at least three of propylene glycol methyl ether propionate, propylene glycol butyl ether, dipropylene glycol dimethyl ether, ethylene glycol butyl ether, dipropylene glycol methyl ether, dimethyl sulfoxide, N-methylpyrrolidone, dipropylene glycol butyl ether or diethylene glycol monobutyl ether; The second cosolvent is at least one of propylene glycol methyl ether acetate, propylene glycol methyl ether acrylate, propylene carbonate, propylene glycol diacetate, ethylene glycol butyl ether acetate, dibasic acid ester or dipropylene glycol dimethyl ether; The surfactant is a Gemini acetylenic diol surfactant; The substrate wetting agent is a polyether-modified silicone surfactant; The aqueous ultraviolet absorber is at least one of BASF Tinuvin 5151, Zhonghao Chemical UV-DL2, Everlight Chemical EVERSORB AQ1, Everlight Chemical EVERSORB AQ2 or Everlight Chemical EVERSORB AQ3; The neutralizing agent is an aqueous solution of 8wt% to 12wt% dimethylethanolamine; The thickener is a polyurethane associative thickener.
7. The method for preparing the water-based topcoat varnish according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1, weighing each raw material according to the designed ratio, adding an aqueous hydroxyl-containing acrylate dispersion, an aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50°C, and an aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5°C into water, mixing evenly, adding a surfactant, a defoamer, a substrate wetting agent, a leveling agent, an aqueous ultraviolet absorber and a first cosolvent, mixing evenly, and then adding a neutralizer and a thickener in sequence, mixing evenly, to obtain component A; S2, adding the second co-solvent into the curing agent, mixing evenly, to obtain component B.
8. Use of the water-based topcoat varnish according to any one of claims 1 to 6 or the water-based topcoat varnish prepared by the preparation method of the water-based topcoat varnish according to claim 7 in automotive coatings.
9. A method for using the water-based top varnish according to any one of claims 1 to 6 or the water-based top varnish prepared by the method for preparing the water-based top varnish according to claim 7, characterized in that: The following steps are involved: Mix component A and component B evenly, add an activated diluent, mix evenly to obtain a construction coating, and evenly apply it on the water-based base paint; The activated diluent comprises an aqueous hydroxyl-containing acrylate dispersion, an aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50° C., an aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5° C., a water-based synthetic sheet silicate solution, a water-based modified urea solution, a first cosolvent, a stabilizer, a defoamer, a leveling agent and water.
10. The method for using the water-based finishing varnish according to claim 9, characterized in that: The activated diluent comprises the following raw material components in mass percentage: 8% to 11.5% of aqueous hydroxyl-containing acrylate dispersion, 3% to 4.5% of aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50°C, 3% to 4.5% of aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5°C, 25% to 33.5% of water-based synthetic sheet silicate solution, 0.5% to 0.7% of water-based modified urea solution, 7.5% to 8.5% of a first cosolvent, 7.5% to 8.5% of a stabilizer, 0.5% to 0.7% of a defoamer, 0.5% to 0.7% of a leveling agent, and 27% to 42% of water, the sum of the components being 100%; The mass ratio of the A component to the activated diluent is 100:(20-30); The water-based synthetic sheet silicate solution comprises the following raw material components in mass percentage: 1.5% to 2.5% of organic modified synthetic sheet silicate, 1.5% to 2.5% of emulsifying dispersant and 95% to 97% of water, the sum of the components being 100%; The water-based modified urea solution is at least one of BYK RHEOBYK-7420CA, BYK RHEOBYK-7420ET or BYK RHEOBYK-7420ES.
Citation Information
Patent Citations
One-component water-based solid color paint for car and preparation process of the one-component water-based solid color paint
CN104592882A
Environment friendly water paint for outer wall of natural gas heat supply pipeline
CN108659651A
Waterborne polyurethane finish paint and preparation method thereof
CN110746875A
Aqueous binder composition
CN110869396A
Waterborne polyurethane waterproof coating material with anti-sagging function
CN113845828A
Cited By
Water-based self-adhesive paint for low-temperature quick-drying direct-welding type high-viscosity enameled wire and preparation method of water-based self-adhesive paint
CN120966355A
Low-temperature fast-drying direct-soldering high-adhesion enameled wire water-based self-adhesive varnish and its preparation method
CN120966355B