Polymer elastomer coating and preparation method thereof
By using polyether polyol PPG2000 and diphenylmethane diisocyanate to prepare polymer elastomer coatings and adding flame retardant and other components, the problem of insufficient physical properties of the existing coatings is solved, and excellent tensile strength is achieved. Tear strength and wear resistance, suitable for thermal insulation materials in complex environments.
Patent Information
- Application Number
- CN202411148181.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-12
AI Technical Summary
The existing polymer elastomer coatings have shortcomings in tensile strength, elongation at break and tear strength, which are difficult to meet the needs of some specific application scenarios, especially in the case of high tensile stress, shear forces and tear. In stress occasions.
Component A is prepared by using polyether polyol PPG2000 and diphenylmethane diisocyanate as raw materials, and by adding flame retardants, catalysts, antioxidants, ultraviolet absorbers and other components, combined with precise control of the polymerization reaction, it forms excellent physical properties. polymer elastomer coating.
It significantly improves the tensile strength, elongation of break and tear strength of the coating, enhances wear resistance and aging resistance, ensures that the coating maintains stability and durability in complex environments, and is suitable for thermal insulation materials and other fields.
Smart Images

Figure CN118931354A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of polymer materials, and in particular relates to a polymer elastomer coating and a preparation method thereof. Background Art
[0002] Polymer elastomeric coatings play an indispensable role in multiple industrial fields and daily applications due to their unique combination of properties. Polymer elastomeric coatings can exhibit excellent elasticity, which means that they can quickly return to their original shape after being subjected to external forces. This elastic property enables the coating to resist repeated deformation and stress, thereby maintaining long-term stability and reliability. In the construction field, polymer elastomeric coatings are often used as waterproof materials for floors, roofs and walls. They can resist tiny deformations caused by temperature changes and foundation movement, and maintain structural integrity and sealing. In the automotive manufacturing field, polymer elastomeric coatings are also widely used in car bodies, chassis and suspension systems. They can absorb and reduce shock and vibration, improving ride comfort and safety.
[0003] Although existing polymer elastomer coatings have shown broad application prospects in many fields, they still have certain limitations in terms of physical properties, especially tensile strength, elongation at break and tear strength. These physical properties are crucial to the durability, reliability and durability of the coating in practical applications. First, tensile strength is an important indicator to measure the ability of the coating to resist fracture when subjected to tensile force. High tensile strength means that the coating can withstand greater external forces without being easily damaged. However, the tensile strength of some polymer elastomer coatings is not ideal, which limits their application in situations where high tensile stress needs to be withstand. Second, elongation at break reflects the maximum deformation that the coating can produce during the stretching process. The elongation at break is an indicator of the degree of deformation. A larger elongation at break means that the coating can produce a larger deformation without breaking when stretched, which is crucial for the flexibility and ductility of the coating. However, the elongation at break of some existing polymer elastomer coatings is relatively low, which makes it difficult to meet the needs of some specific application scenarios. In addition, tear strength is also one of the important indicators for evaluating the physical properties of coatings. It reflects the ability of the coating to resist damage when cut or torn by sharp objects. High tear strength can ensure that the coating is not easily torn or damaged when subjected to external physical impact or damage. However, the tear strength of some polymer elastomer coatings still needs to be improved, especially in some occasions that need to withstand high shear force and tear stress.
[0004] Therefore, developing a polymer elastomer coating with excellent physical properties has important practical application value. Summary of the Invention
[0005] In view of the deficiencies of the prior art, the present invention provides a polymer elastomer coating and a preparation method thereof, wherein the coating has excellent tensile strength, elongation at break, tear strength and wear resistance.
[0006] The technical solution provided by the present invention is as follows: The present invention provides a polymer elastomer coating, comprising component A and component B. Component A: a prepolymer with an isocyanate content of 13.5% to 16% obtained by reaction of polyether polyol PPG2000 and diphenylmethane diisocyanate; Component B: including polyether polyol, flame retardant, catalyst, dispersant, defoaming agent, antioxidant, UV absorber, antistatic agent and anti-settling agent; The weight ratio of component A to component B is 1 to 1.5:1.
[0007] Furthermore, component B comprises the following raw materials in the following mass ratios: 80-100 parts of polyether polyol, 5-15 parts of flame retardant, 0.005-0.01 parts of catalyst, 0.15-0.3 parts of dispersant, 0.001-0.03 parts of defoaming agent, 0.5-1.5 parts of antioxidant, 0.3-1.0 parts of ultraviolet absorber, 0.5-5 parts of antistatic agent, and 0.01-0.05 parts of anti-settling agent.
[0008] Furthermore, component A comprises the following raw materials in the following mass ratios: 45 to 60 parts of polyether polyol PPG2000 and 50 parts of diphenylmethane diisocyanate.
[0009] Furthermore, the polyether polyol in the B component is a mixture of polyether triol and polyether diol, the volume ratio of the polyether triol to the polyether diol is 5:0.6-3, and the number average molecular weight is 2000-5000.
[0010] Furthermore, the catalyst in the B component is an organic tin catalyst or an amine catalyst.
[0011] Furthermore, the organotin catalyst is selected from any one or more of stannous octoate, dibutyltin dilaurate, dibutyltin didodecylsulfide, dibutyltin diacetate, dibutyltin dioctoate, tin (II) acetate, tin (II) octoate, tin ethylhexanoate, tin laurate, dibutyltin oxide, dibutyltin dichloride, dibutyltin diacetate, dibutyltin maleate, and dioctyltin diacetate.
[0012] Furthermore, the amine catalyst is selected from any one or more of triethylamine, tributylamine, triethylenediamine, N-ethylmorpholine, N,N,N',N'-tetramethyl-ethylenediamine, N,N-methylaniline, N,N-dimethylaniline, N,N,N',N",N"-pentamethyldiethylenetriamine, and bis(2-dimethylaminoethyl) ether.
[0013] Furthermore, the flame retardant in the B component is selected from any one or more of ammonium polyphosphate APP, melamine polyphosphate MPP, ammonium phosphate, phosphaphenanthrene DOPO, phosphazene compounds, organic phosphinic acid, and organic phosphinic acid salts.
[0014] Furthermore, the ultraviolet absorber in the B component is selected from any one or more of phenyl o-hydroxybenzoate, 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, and 4-benzoyloxy-2,2,6,6-tetramethylpiperidine.
[0015] The present invention also provides a method for preparing the polymer elastomer coating described above, the method comprising the following steps: S1. Preparation of Component A: Dehydrate polyether polyol PPG2000 at 100°C to 105°C and vacuum at -0.08 MPa to -0.1 MPa for 2.5 to 3.5 hours under stirring; add diphenylmethane diisocyanate after cooling the above materials to 50°C to 70°C, react at 80°C to 85°C for 2.0 to 2.5 hours, and then cool to 50°C to 60°C to obtain Component A, wherein the content of isocyanate groups in Component A is 13.5% to 16%; S2. Preparation of component B: Under stirring, dehydrate the polyether polyol, flame retardant, catalyst, dispersant, defoaming agent, antioxidant, UV absorber and antistatic agent in a vacuum environment of 100° C. to 105° C. and -0.08 MPa to -0.1 MPa for 2.0 to 3.0 hours; after the mixture is cooled to 50° C. to 60° C., continue to disperse and add the anti-settling agent, and disperse and stir for 30 minutes to 50 minutes to obtain component B; S3. Mix the materials of component A and component B to obtain a polymer elastomer coating. Beneficial effects
[0016] The polymer elastomer coating of the present invention adopts an efficient and specially selected catalyst during the preparation process of the coating. This catalyst effectively promotes the formation and cross-linking of polymer chains by precisely controlling the rate and path of the polymerization reaction, thereby significantly improving the overall performance of the coating. The catalytic acceleration of the reaction not only improves production efficiency, but also ensures the stability and consistency of the coating quality. In order to enhance the aging resistance of the coating, the present invention specially adds antioxidants and UV absorbers. The antioxidant can effectively capture and remove free radicals generated in the coating to prevent them from initiating chain reactions, thereby delaying the oxidation and aging process of the coating. The UV absorber can selectively absorb ultraviolet energy and convert it into harmless heat energy release, reducing the destructive effect of ultraviolet rays on the coating. The synergistic effect of these two additives enables the polymer elastomer coating to exhibit better strength and aging resistance in the application of thermal insulation materials.
[0017] The polymer elastomer coating of the present invention focuses on environmental protection performance. No volatile harmful solvents are used in the coating formula, which not only reduces environmental pollution in the production process, but also provides users with a safer and healthier use environment. At the same time, through careful formulation and optimization, in order to ensure that the coating does not produce harmful volatiles during use and is harmless to the environment and human health, the polymer elastomer coating used in the present invention has excellent physical properties, and its tensile strength and tear strength have reached the industry-leading level, which enables the coating to withstand various complex external forces without being easily damaged. In addition, the coating also has excellent wear resistance and corrosion resistance, and can maintain long-term stability and durability under harsh environmental conditions. These excellent physical properties enable the coating to permanently protect the insulation material from damage, providing users with reliable protection.
[0018] In summary, the polymer elastomer coating of the present invention achieves excellent application in the field of thermal insulation materials by adopting catalytic acceleration reaction, adding antioxidants and ultraviolet absorbers, and optimizing environmental performance and physical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is a preparation flow chart of the polymer elastomer coating of the present invention. DETAILED DESCRIPTION
[0020] The following will clearly and completely describe the technical solutions in the embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.
[0021] The embodiment of the present invention provides a polymer elastomer coating, comprising component A and component B. Component A: a prepolymer with an isocyanate content of 13.5% to 16% obtained by reaction of polyether polyol PPG2000 and diphenylmethane diisocyanate; Component B: including polyether polyol, flame retardant, catalyst, dispersant, defoaming agent, antioxidant, UV absorber, antistatic agent and anti-settling agent; The weight ratio of component A to component B is 1 to 1.5:1.
[0022] In this embodiment, component B comprises the following raw materials in the following mass ratios: 80-100 parts of polyether polyol, 5-15 parts of flame retardant, 0.005-0.01 parts of catalyst, 0.15-0.3 parts of dispersant, 0.001-0.03 parts of defoaming agent, 0.5-1.5 parts of antioxidant, 0.3-1.0 parts of ultraviolet absorber, 0.5-5 parts of antistatic agent, and 0.01-0.05 parts of anti-settling agent.
[0023] In this embodiment, component A comprises the following raw materials in the following mass ratios: 45 to 60 parts of polyether polyol PPG2000 and 50 parts of diphenylmethane diisocyanate.
[0024] In this embodiment, the polyether polyol in the B component is a mixture of polyether triol and polyether diol, the volume ratio of the polyether triol to the polyether diol is 5:0.6-3, and the number average molecular weight thereof is 2000-5000.
[0025] In this embodiment, the catalyst in the component B is an organotin catalyst or an amine catalyst.
[0026] In this embodiment, the organotin catalyst is selected from any one or more of stannous octoate, dibutyltin dilaurate, dibutyltin didodecylsulfide, dibutyltin diacetate, dibutyltin dioctoate, tin (II) acetate, tin (II) octoate, tin ethylhexanoate, tin laurate, dibutyltin oxide, dibutyltin dichloride, dibutyltin diacetate, dibutyltin maleate, and dioctyltin diacetate.
[0027] In this embodiment, the amine catalyst is selected from any one or more of triethylamine, tributylamine, triethylenediamine, N-ethylmorpholine, N,N,N',N'-tetramethyl-ethylenediamine, N,N-methylaniline, N,N-dimethylaniline, N,N,N',N",N"-pentamethyldiethylenetriamine, and bis(2-dimethylaminoethyl) ether.
[0028] Specifically, the catalyst in this embodiment is dibutyltin dioctoate.
[0029] In this embodiment, the flame retardant in the B component is selected from any one or more of ammonium polyphosphate APP, melamine polyphosphate MPP, ammonium phosphate, phosphaphenanthrene DOPO, phosphazene compounds, organic phosphinic acid, and organic phosphinic acid salts.
[0030] Specifically, the flame retardant is a mixture of melamine polyphosphate MPP and ammonium phosphate, and the mass ratio of melamine polyphosphate MPP to ammonium phosphate is 1:1.
[0031] In this embodiment, the ultraviolet absorber in the B component is selected from any one or more of phenyl o-hydroxybenzoate, 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, and 4-benzoyloxy-2,2,6,6-tetramethylpiperidine.
[0032] Specifically, the ultraviolet light absorber is a mixture of 2,4-dihydroxybenzophenone and 4-benzoyloxy-2,2,6,6-tetramethylpiperidine, and the mass ratio of 2,4-dihydroxybenzophenone to 4-benzoyloxy-2,2,6,6-tetramethylpiperidine is 1:2.
[0033] An embodiment of the present invention further provides a method for preparing the polymer elastomer coating described above, the method comprising the following steps: S1. Preparation of Component A: Dehydrate polyether polyol PPG2000 at 100°C to 105°C and vacuum at -0.08 MPa to -0.1 MPa for 2.5 to 3.5 hours under stirring; add diphenylmethane diisocyanate after cooling the above materials to 50°C to 70°C, react at 80°C to 85°C for 2.0 to 2.5 hours, and then cool to 50°C to 60°C to obtain Component A, wherein the content of isocyanate groups in Component A is 13.5% to 16%; S2. Preparation of component B: Under stirring, dehydrate the polyether polyol, flame retardant, catalyst, dispersant, defoaming agent, antioxidant, UV absorber and antistatic agent in a vacuum environment of 100° C. to 105° C. and -0.08 MPa to -0.1 MPa for 2.0 to 3.0 hours; after the mixture is cooled to 50° C. to 60° C., continue to disperse and add the anti-settling agent, and disperse and stir for 30 minutes to 50 minutes to obtain component B; S3. Mix the materials of component A and component B to obtain a polymer elastomer coating.
[0034] The following is a detailed description of a polymer elastomer coating and a preparation method provided by the present invention in conjunction with the embodiments. Figure 1 ), but they should not be understood as limiting the scope of protection of the present invention.
[0035] Example 1
[0036] 1. Material Preparation
[0037] Before preparing a polymer elastomer coating, the necessary raw materials must be prepared. For component A, polyether polyol PPG2000 and diphenylmethane diisocyanate are selected as the primary raw materials. Polyether polyol PPG2000 has an appropriate molecular weight and chemical stability, making it suitable for preparing high-performance elastomer coatings. For component B, various additives are required, including polyether polyol, flame retardant, catalyst, dispersant, defoamer, antioxidant, UV absorber, antistatic agent, and anti-settling agent.
[0038] 2. Preparation of Component A
[0039] Dehydration treatment:
[0040] Under stirring, a certain amount of polyether polyol PPG2000 is placed into the reactor.
[0041] Heat the reactor to 100-105°C and simultaneously evacuate to -0.08-0.1 MPa to remove moisture and impurities from the polyether polyol. This process lasts 2.5-3.5 hours to ensure full dehydration of the polyether polyol.
[0042] Isocyanate reaction:
[0043] When the temperature of the polyether polyol drops to 50°C to 70°C, add a certain amount of diphenylmethane diisocyanate MDI-50.
[0044] The reaction is carried out at a temperature of 80° C. to 85° C. for 2.0 to 2.5 hours to allow the isocyanate group (-NCO) to react with the hydroxyl group (-OH) in the polyether polyol to form a polyurethane prepolymer.
[0045] After the reaction is completed, the temperature is lowered to 50°C to 60°C to obtain component A. By adjusting the reaction conditions and the ratio of raw materials, the content of isocyanate groups (-NCO) in component A is controlled to be 13.5%, and the weight ratio of polyether polyol to diphenylmethane diisocyanate is controlled to be 0.885:1.
[0046] 3. Preparation of component B
[0047] Mixing and dehydration:
[0048] Under stirring, 80 parts of polyether polyol, 15 parts of flame retardant, 0.005 parts of catalyst, 0.3 parts of dispersant, 0.03 parts of defoaming agent, 0.5 parts of antioxidant, 1.0 parts of ultraviolet absorber and 0.5 parts of antistatic agent are mixed in a certain proportion, and the volume ratio of polyether triol and polyether diol is 5:1.2.
[0049] The mixture is heated to 100° C. to 105° C. and simultaneously evacuated to -0.08 MPa to -0.1 MPa for dehydration treatment for 2.0 to 3.0 hours to remove moisture and impurities in the raw materials.
[0050] Dispersion and stirring:
[0051] When the mixture is cooled to 50°C to 60°C, 0.01 parts of anti-settling agent is added.
[0052] The dispersion mixer is used to disperse and stir for 30 to 50 minutes to ensure that all the raw materials are fully mixed to obtain component B.
[0053] 4. Mixing of components A and B
[0054] Mix component A and component B in a certain ratio (such as 1 to 1.5:1) at the construction site.
[0055] Through proper stirring and mixing methods, ensure that components A and B are fully mixed and evenly mixed to form a polymer elastomer coating.
[0056] Through the detailed preparation process of Example 1, a polymeric elastomeric coating with excellent physical properties and chemical stability was prepared. This coating not only exhibits excellent tensile strength, elongation at break, and tear strength, but also exhibits good aging resistance and environmental performance. Furthermore, the addition of additives such as flame retardants, antioxidants, and UV absorbers further enhances the coating's safety and durability. This polymeric elastomeric coating has broad application prospects in fields such as thermal insulation materials.
[0057] Example 2
[0058] 1. Material Preparation
[0059] This example provides a polymeric elastomeric coating composed of two components, A and B. Component A is primarily based on the reaction of polyether polyol PPG2000 and diphenylmethane diisocyanate, while component B contains various additives to provide the desired functionality and stability. The preparation of these two components and the final mixing step are described in detail below.
[0060] 2. Preparation of Component A
[0061] Dehydration treatment:
[0062] While stirring, place a certain amount of polyether polyol PPG2000 in a reactor, heat the reactor to 100°C to 105°C, and simultaneously evacuate the reactor to a pressure of -0.08MPa to -0.1MPa. This process lasts for 2.5 to 3.5 hours to fully remove moisture and impurities from the polyether polyol.
[0063] Isocyanate reaction:
[0064] After the dehydrated polyether polyol is cooled to 50°C to 70°C, a certain amount of diphenylmethane diisocyanate (MDI-50) is added. Subsequently, the reaction is carried out at 80°C to 85°C for 2.0 to 2.5 hours to allow the isocyanate groups (-NCO) to react with the hydroxyl groups (-OH) in the polyether polyol to form a polyurethane prepolymer. After the reaction is completed, the temperature is lowered to 50°C to 60°C to obtain Component A. By precisely controlling the reaction conditions and raw material ratios, the isocyanate group (-NCO) content in Component A is ensured to reach the predetermined 14%. The weight ratio of polyether polyol to diphenylmethane diisocyanate is 0.93:1.
[0065] 3. Preparation of component B
[0066] Raw material mixing and dehydration:
[0067] Under stirring, 100 parts of polyether polyol, 15 parts of flame retardant, 0.01 parts of catalyst, 0.3 parts of dispersant, 0.03 parts of defoaming agent, 0.5 parts of antioxidant, 1.0 parts of ultraviolet absorber and 0.5 parts of antistatic agent are mixed in a certain proportion, wherein the volume ratio of polyether triol and polyether diol is 5:1.0.
[0068] Subsequently, the mixture is placed in an environment of 100° C. to 105° C. and a vacuum of -0.08 MPa to -0.1 MPa for dehydration for 2.0 to 3.0 hours to remove moisture and impurities in the raw materials.
[0069] Dispersion and stirring:
[0070] After the dehydrated mixture is cooled to 50°C to 60°C, 0.01 parts of an anti-settling agent is added and dispersed in a dispersing mixer for 30 to 50 minutes to ensure that all the raw materials are fully mixed to obtain component B.
[0071] 4. Mixing of components A and B
[0072] Mix the prepared components A and B at a certain ratio (e.g., 1-1.5:1) at the construction site. Ensure that components A and B are fully mixed and evenly mixed through appropriate stirring and mixing methods to form a polymer elastomer coating.
[0073] Through the detailed preparation process of Example 2, a polymeric elastomeric coating with excellent physical properties and chemical stability was prepared. This coating not only exhibits excellent tensile strength, elongation at break, and tear strength, but also exhibits good aging resistance and environmental performance. Furthermore, the addition of additives such as flame retardants, antioxidants, and UV absorbers further enhances the coating's safety and durability. This polymeric elastomeric coating has broad application prospects in thermal insulation materials, architectural coatings, waterproof coatings, and other fields.
[0074] Example 3
[0075] 1. Material Preparation
[0076] This example describes in detail the preparation of a polymeric elastomeric coating composed of two components, A and B. Component A is based on the reaction of polyether polyol PPG2000 and diphenylmethane diisocyanate, while component B is a mixture of various additives designed to enhance the coating's functionality and stability. The following details the preparation steps for these two components and the final mixing process.
[0077] 2. Preparation of Component A
[0078] Dehydration treatment:
[0079] First, a certain amount of polyether polyol PPG2000 is placed in a reaction vessel while stirring. The vessel is then heated to 100°C to 105°C and dehydrated under a vacuum of -0.08MPa to -0.1MPa for 2.5 to 3.5 hours. This step removes moisture and impurities from the polyether polyol, ensuring smooth subsequent reactions.
[0080] Isocyanate reaction:
[0081] When the polyether polyol is cooled to 50°C to 70°C, a certain amount of diphenylmethane diisocyanate (MDI-50) is added. The reaction is then carried out at a temperature of 80°C to 85°C for 2.0 to 2.5 hours. During this process, the isocyanate groups (-NCO) react with the hydroxyl groups (-OH) in the polyether polyol to form a polyurethane prepolymer. After the reaction is completed, the temperature is lowered to 50°C to 60°C to obtain component A. By precisely controlling the reaction conditions and raw material ratios, the isocyanate group (-NCO) content in component A is ensured to reach the predetermined 15%. The weight ratio of polyether polyol to diphenylmethane diisocyanate is 1.03:1.
[0082] 3. Preparation of component B
[0083] Raw material mixing and dehydration:
[0084] While stirring, 100 parts of polyether polyol, 10 parts of flame retardant, 0.008 parts of catalyst, 0.3 parts of dispersant, 0.03 parts of defoaming agent, 0.05 parts of antioxidant, 1.0 parts of UV absorber, and 0.5 parts of antistatic agent were mixed in a certain proportion. The volume ratio of polyether triol to polyether diol was 5:0.8.
[0085] The mixture is then placed in a dehydration process at 100°C to 105°C and a vacuum of -0.08 MPa to -0.1 MPa for 2.0 to 3.0 hours. This step aims to remove moisture and impurities from the raw materials and ensure the stability and functionality of component B.
[0086] Dispersion and stirring:
[0087] After the dehydrated mixture is cooled to 50-60°C, 0.01 part of an anti-settling agent is added. Then, the mixture is dispersed and stirred in a dispersing mixer for 30-50 minutes to ensure that all the raw materials are fully mixed to obtain component B.
[0088] 4. Mixing of components A and B
[0089] Mix the prepared components A and B at a certain ratio (e.g., 1-1.5:1) at the construction site. Ensure that components A and B are fully mixed and evenly mixed through appropriate stirring and mixing methods to form a polymer elastomer coating.
[0090] Through the detailed preparation process of Example 3, a polymeric elastomeric coating with excellent physical properties and chemical stability was prepared. The precise preparation of component A ensures the coating possesses excellent elasticity and strength, while the addition of various additives to component B further enhances the coating's flame retardancy, oxidation resistance, UV resistance, and antistatic properties. This polymeric elastomeric coating has broad application prospects in thermal insulation materials, architectural coatings, waterproof coatings, and other fields.
[0091] The polymer elastomer coatings prepared in Examples 1-3 were subjected to performance tests according to national standards. The test results are shown in Table 1.
[0092] Table 1 Properties of the polymer elastomer coatings prepared in Example
[0093]
[0094] As shown in the table above, the isocyanate group (-NCO) content in component A represents the hard end of the elastomer material. As the isocyanate group (-NCO) content increases, the material's strength gradually increases. Increasing the volume ratio of the polyether triol to the polyether diol in component B leads to increasingly higher tensile strength in the coating. By combining these two components, the material achieves significant improvements in tensile strength, tear strength, and abrasion resistance. This is of great significance for improving the material's performance and applicability, and also provides valuable insights for further research and application in materials science.
[0095] The anti-corrosion performance test of the polymer elastomer coating prepared in Example 3 was carried out in accordance with the national standard (GB / T16777-2008). It was found that the tensile strength retention rate after 720h of artificial weathering was 90%, the tensile strength retention rate after 720h of alkali treatment was 82%, and the tensile strength retention rate after 720h of acid treatment was 85%. There was no cracking when bent at -40°C.
[0096] In summary, the polymer elastomer coating of the present invention can be applied to the field of thermal insulation materials by adopting catalytic acceleration reaction, adding antioxidants and ultraviolet absorbers, and optimizing environmental performance and physical properties.
Claims
1. A polymer elastomer coating, comprising component A and component B, characterized in that: Component A: a prepolymer with an isocyanate mass content of 13.5% to 16% obtained by reaction of polyether polyol PPG2000 and diphenylmethane diisocyanate as raw materials; Component B: including polyether polyol, flame retardant, catalyst, dispersant, defoamer, antioxidant, UV absorber, antistatic agent and anti-settling agent; The weight ratio of the component A to the component B is 1 to 1.5:
1.
2. The polymer elastomer coating according to claim 1, characterized in that: Component B comprises the following raw materials in the following mass ratios: 80-100 parts of polyether polyol, 5-15 parts of flame retardant, 0.005-0.01 parts of catalyst, 0.15-0.3 parts of dispersant, 0.001-0.03 parts of defoaming agent, 0.5-1.5 parts of antioxidant, 0.3-1.0 parts of ultraviolet absorber, 0.5-5 parts of antistatic agent and 0.01-0.05 parts of anti-settling agent.
3. The polymer elastomer coating according to claim 1, characterized in that: Component A comprises the following raw materials in the following mass ratios: 45 to 60 parts of polyether polyol PPG2000 and 50 parts of diphenylmethane diisocyanate.
4. The polymer elastomer coating according to claim 1, characterized in that: The polyether polyol in the B component is a mixture of polyether triol and polyether diol, the volume ratio of the polyether triol to the polyether diol is 5:0.6-3, and the number average molecular weight is 2000-5000.
5. The polymer elastomer coating according to claim 1, characterized in that: The catalyst in the B component is an organic tin catalyst or an amine catalyst.
6. The polymer elastomer coating according to claim 5, characterized in that: The organotin catalyst is selected from any one or more of stannous octoate, dibutyltin dilaurate, dibutyltin didodecylsulfide, dibutyltin diacetate, dibutyltin dioctoate, tin (II) acetate, tin (II) octoate, tin ethylhexanoate, tin laurate, dibutyltin oxide, dibutyltin dichloride, dibutyltin diacetate, dibutyltin maleate, and dioctyltin diacetate.
7. The polymer elastomer coating according to claim 5, characterized in that: The amine catalyst is selected from any one or more of triethylamine, tributylamine, triethylenediamine, N-ethylmorpholine, N,N,N',N'-tetramethyl-ethylenediamine, N,N-methylaniline, N,N-dimethylaniline, N,N,N',N",N"-pentamethyldiethylenetriamine, and bis(2-dimethylaminoethyl) ether.
8. The polymer elastomer coating according to claim 1, characterized in that: The flame retardant in the B component is selected from any one or more of ammonium polyphosphate APP, melamine polyphosphate MPP, ammonium phosphate, phosphaphenanthrene DOPO, phosphazene compounds, organic phosphinic acid, and organic phosphinates.
9. The polymer elastomer coating according to claim 1, characterized in that: The ultraviolet absorber in the B component is selected from any one or more of phenyl o-hydroxybenzoate, 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, and 4-benzoyloxy-2,2,6,6-tetramethylpiperidine.
10. A method for preparing a polymer elastomer coating according to any one of claims 1 to 9, characterized in that: The preparation method comprises the following steps: S100, preparing component A: under stirring, dehydrate polyether polyol PPG2000 at 100°C to 105°C and vacuum environment of -0.08MPa to -0.1MPa for 2.5 to 3.5 hours; after cooling the above materials to 50°C to 70°C, add diphenylmethane diisocyanate, react at 80°C to 85°C for 2.0 to 2.5 hours, and then cool to 50°C to 60°C to obtain component A, wherein the content of isocyanate groups in component A is 13.5% to 16%; S200, preparing component B: under stirring, placing polyether polyol, flame retardant, catalyst, dispersant, defoamer, antioxidant, ultraviolet absorber and antistatic agent in a vacuum environment of -0.08MPa to -0.1MPa at 100°C to 105°C for dehydration for 2.0 to 3.0 hours; after the mixture is cooled to 50°C to 60°C, the anti-settling agent is continuously dispersed and added, and the dispersion and stirring are performed for 30min to 50min to obtain component B; S300, mixing the materials of component A and component B to obtain a polymer elastomer coating.
Citation Information
Patent Citations
Highly-elastic urethane elastomer composition
CN101134843A
Bicomponent high-strength sprayed polyurethane waterproof paint
CN101608094A
Elastomer composition material for polyurethane spraying material and preparation method thereof
CN104178015A
Polyurethane type spraying elastomer and preparation method thereof
CN110922884A
Preparation method of rapid repairing material for rubber belt
CN113249022A