Anti-rust and anti-corrosion coating for electric power iron tower and preparation method thereof
Through the coordinated anti-corrosion effect of modified water-based polyurethane, modified epoxy resin and mesoporous nano zinc molybdate/zinc phosphate and other materials, the problem of insufficient weather resistance and chemical solvent resistance of the electric tower in environmental corrosion is solved, and a A high-performance, green and environmentally friendly water-based anti-rust and anti-corrosion coating suitable for power towers.
Patent Information
- Application Number
- CN202411239659.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-05
AI Technical Summary
Electric towers are prone to corrosion under various environmental conditions. The existing anti-rust and corrosion-resistant coatings have shortcomings in weather resistance, chemical solvent resistance and salt spray resistance, and traditional coatings have problems with environmental pollution and the use of toxic materials.
Using modified water-based polyurethane, modified epoxy resin and mesoporous nano zinc molybdate/zinc phosphate and other materials, a water-based power tower anti-rust and anti-corrosion coating is prepared through physical and chemical synergistic anti-corrosion effects, combining nano-silica and oxidation. Graphene improves the corrosion resistance and environmental protection of the paint.
It achieves high water resistance, acid and alkali resistance, salt spray resistance and impact resistance of the paint, and has good rust resistance. It is suitable for power towers and meets the needs of green and environmental protection and high performance.
Smart Images

Figure BDA0005028849860000161
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coatings, and in particular to an anti-rust and anti-corrosion coating for an electric power tower and a preparation method thereof. Background Art
[0002] Power towers are susceptible to corrosion due to long-term exposure to various environmental conditions, so anti-rust and anti-corrosion coatings are needed to extend their service life. According to the search results, Shandong Electric Power Research Institute has developed a new type of anti-rust and anti-corrosion coating.
[0003] Anticorrosion coatings should be classified as functional (special) coatings. Since the liberation of my country, anticorrosion coatings have been given great attention. They have roughly gone through three periods of development. In the first period, oily resins, alkyd resins, and phenolic resins were mostly used as base materials. Anticorrosion pigments also used red lead and other lead and chromium pigments as antirust components. This period roughly extended to the 1960s. Since then, synthetic resins have been developed. In addition to the above-mentioned base materials, there are also epoxy, chlorinated rubber, vinyl resin, chlorosulfonated polyethylene, silicate, etc. Anticorrosion pigments also include zinc powder, aluminum powder, zinc phosphate, barium metaborate, red iron oxide and other non-toxic varieties. Rheological additives began to be used in anticorrosion coatings, and heavy anticorrosion coatings appeared. The wet adhesion theory and barrier principle were also used in anticorrosion coatings. Due to the increasingly stringent requirements for environmental protection, replacing the original base materials that pollute the atmosphere and the toxic antirust pigments that harm the environment has become the main direction for the development of new anticorrosion coatings. At the same time, various industries and construction fields have put forward new requirements for anticorrosion coatings, especially heavy anticorrosion. These include the need for high performance, economy, adaptability to poor substrates or rusty coatings, no heavy metals, high solids, water-based or solvent-free, ultra-thick film type, odorless, anti-corrosion and decorative, acid rain resistance, multi-function, energy saving, etc. These are the main goals of the current development of anti-corrosion coatings in my country. Summary of the invention
[0004] The purpose of the present invention is to propose an anti-rust and anti-corrosion coating for an electric power tower and a preparation method thereof, so as to improve the anti-corrosion performance of the coating through physical and chemical synergistic anti-corrosion effects. At the same time, the coating is a water-based coating, which is green and environmentally friendly, has good flexibility, impact resistance, chemical solvent resistance, weather resistance, and salt spray resistance, has good anti-rust performance, and has broad application prospects.
[0005] The technical solution of the present invention is achieved in this way:
[0006] The invention provides a method for preparing an anti-rust and anti-corrosion coating for an electric power tower. The method comprises the following steps: modifying polyurethane with piceatannol and resveratrol to prepare a modified waterborne polyurethane; modifying graphene oxide with polydopamine, adding the graphene oxide and nano silicon dioxide into epoxy resin to prepare a modified epoxy resin emulsion; preparing mesoporous nano zinc molybdate / zinc phosphate, modifying the surface with a silane coupling agent, and then stirring and mixing the modified waterborne polyurethane, the modified epoxy resin emulsion, a pH value regulator, a dispersant, a defoamer, a pigment, talcum powder and water to uniformly mix the mixture; performing a colloid mill, adding a thickener, stirring and filtering the mixture, and preparing the anti-rust and anti-corrosion coating for an electric power tower.
[0007] As a further improvement of the present invention, the following steps are included:
[0008] S1. Preparation of a modifier: mixing piceatannol and resveratrol uniformly to prepare a modifier;
[0009] S2. Preparation of modified waterborne polyurethane: adding polytetrahydrofuran diol to acetone, heating, adding isocyanate dropwise, stirring to react, adding a catalyst, dimethylol propionic acid, 1,4-butanediol and a modifier, continuing to stir to react, cooling to room temperature, adding triethylamine, stirring to react, adding deionized water, emulsifying, and removing acetone under reduced pressure to obtain a modified waterborne polyurethane;
[0010] S3. Preparation of modified graphene oxide: dissolving graphene oxide in water, adding dopamine hydrochloride and a catalyst, heating and stirring to react, and drying to obtain modified graphene oxide;
[0011] S4. Preparation of modified epoxy resin emulsion: polyethylene glycol and multifunctional epoxy resin are mixed, boron trifluoride ether is added, heated and stirred to react, and an emulsifier is prepared, the emulsifier and epoxy resin are added to water, heated and stirred to react, and then modified graphene oxide and nano-silica are added, stirred to react, and colloid milled to prepare a modified epoxy resin emulsion;
[0012] S5. Preparation of mesoporous nano zinc molybdate / zinc phosphate: dissolve ammonium molybdate and ammonium phosphate in water, add ethanol and polyethylene glycol, stir and mix evenly, dropwise add zinc chloride solution, then add polyvinyl alcohol, heat and stir to react, centrifuge, wash, and dry to obtain mesoporous nano zinc molybdate / zinc phosphate;
[0013] S6. Preparation of modified mesoporous nano zinc molybdate / zinc phosphate: adding mesoporous nano zinc molybdate / zinc phosphate to ethanol, adding a silane coupling agent, heating and stirring to react, to obtain modified mesoporous nano zinc molybdate / zinc phosphate;
[0014] S7. Preparation of anti-rust and anti-corrosion coating for power tower: Stir and mix modified waterborne polyurethane, modified epoxy resin emulsion, pH adjuster, dispersant, defoaming agent and water evenly, add modified mesoporous nano zinc molybdate / zinc phosphate, pigment and talcum powder, colloid mill, add thickener, stir evenly, filter, and obtain the anti-rust and anti-corrosion coating for power tower.
[0015] As a further improvement of the present invention, the mass ratio of piceatannol to resveratrol in step S1 is 3-5:2-3.
[0016] As a further improvement of the present invention, the mass ratio of the polytetrahydrofuran diol, isocyanate, catalyst, dimethylol propionic acid, 1,4-butanediol, modifier and triethylamine in step S2 is 10: 5-7: 0.01-0.02: 1-2: 0.2-0.4: 2-4: 0.5-1.5, the heating temperature is 55-65°C, the isocyanate is selected from at least one of isophorone diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, hexamethylene diisocyanate and lysine diisocyanate, the catalyst is dibutyltin dilaurate or stannous octoate, and the emulsification time is 20-30 min.
[0017] As a further improvement of the present invention, the mass ratio of graphene oxide, dopamine hydrochloride and catalyst in step S3 is 10:3-6:0.1-0.2, the temperature of the heating and stirring reaction is 40-50°C, the time is 2-4h, and the catalyst is a Tris-HCl solution with a pH of 8.5-9.5.
[0018] As a further improvement of the present invention, the mass ratio of the polyethylene glycol, the multifunctional epoxy resin, and the boron trifluoride ether in step S4 is 3-5:4-7:0.5-1, the multifunctional epoxy resin is the epoxy resin DEN-425, the mass ratio of the emulsifier, the epoxy resin, the modified graphene oxide, and the nano-silicon dioxide is 2-4:60-80:4-7:1-2, the rotation speed of the colloid mill is 10000-12000r / min, the time is 1-3h, and the epoxy resin is bisphenol A or bisphenol F type epoxy resin.
[0019] As a further improvement of the present invention, the mass ratio of ammonium molybdate, ammonium phosphate, ethanol, polyethylene glycol, zinc chloride and polyvinyl alcohol in step S5 is 1.9-2.0:1.4-1.5:10-15:0.3-0.5:2.6-2.8:0.1-0.2, and the temperature of the heating and stirring reaction is 55-65°C and the time is 1-2h.
[0020] As a further improvement of the present invention, the mass ratio of the mesoporous nano zinc molybdate / zinc phosphate and the silane coupling agent in step S6 is 10:1-2, the silane coupling agent is selected from at least one of KH550, KH692, and KH702, and the temperature of the heating and stirring reaction is 40-50°C and the time is 1-3h.
[0021] As a further improvement of the present invention, the mass ratio of the modified waterborne polyurethane, modified epoxy resin emulsion, pH regulator, dispersant, defoamer, water, modified mesoporous nano zinc molybdate / zinc phosphate, pigment, talcum powder and thickener in step S7 is 30-40:7-10:1-2:0.2-0.4:0.1-0.2:20-40:3-4:1-3:1-2:0.5-1, the pH regulator is N,N-dimethylethanol, the dispersant is 104BC, the defoamer is BYK-024, the pigment is carbon black, and the thickener is polyurethane RM-8W.
[0022] The present invention further protects an anti-rust and anti-corrosion coating for an electric power tower prepared by the above-mentioned preparation method.
[0023] The present invention has the following beneficial effects:
[0024] Compared with traditional solvent-based polyurethane coatings, water-based polyurethane coatings are insufficient in water resistance, chemical resistance, heat resistance and fullness. The present invention uses piceatannol and resveratrol as internal cross-linking modifiers, which have both conjugated double bonds and hydroxyl structures and can react with isocyanate to form polyurethane segments with branches, which not only play the role of internal cross-linking agents, but also the conjugated double bonds can be oxidized and cross-linked to form films, so that the water-based emulsion has better film-forming properties, thereby improving the water resistance, acid and alkali resistance and salt spray resistance of the water-based polyurethane anti-corrosion coating film.
[0025] Compared with other resins such as polyurethane and silicone, epoxy resin has better anti-corrosion protection, but it is insufficient in toughness and impact resistance. Graphene is an emerging two-dimensional nanomaterial with excellent conductivity, flexibility, and physical shielding properties of water molecules and air, but the easy aggregation of graphene makes it difficult to evenly disperse in epoxy resin emulsion. The present invention modifies graphene oxide by polydopamine, and the amino groups on its surface can react with the residual epoxy groups of epoxy resin, thereby improving the dispersibility of graphene oxide, solving the agglomeration problem caused by physical blending and adding graphene, and achieving a strong physical shielding effect given to the coating with a small amount of graphene. At the same time, it also greatly improves the flexibility, conductivity and impact resistance of the coating.
[0026] Zinc phosphate is an environmentally friendly anti-rust pigment with excellent performance, but ordinary zinc phosphate has a large particle size, a small specific surface area, a low solubility in water, poor hydrolysis, and a slow speed of forming a passivation protective film in the early stage of corrosion, thereby affecting the overall anti-rust performance of the coating. The present invention also prepares a mesoporous nano zinc molybdate / zinc phosphate, which greatly reduces the particle size of the product, and the mesoporous structure and nano-scale particles increase its specific surface area. The product is further modified by a silane coupling agent with an amino group, and the obtained product can react with the residual groups of isocyanate and epoxy resin, thereby improving the dispersibility of the product and avoiding adverse effects on mechanical properties. At the same time, zinc phosphate and zinc molybdate produce local anodes and cathodes on the surface of steel in the early stage of corrosion, and zinc phosphate hydrolyzes the dissolved iron salts and ferrous salts, and the released protons react with zinc phosphate to produce phosphoric acid and zinc ions, and the zinc ions and iron ions are insoluble complexes on site to precipitate Fe[Zn3(PO4)], which plays a role in cathode protection. Zinc molybdate can not only form complexes with iron ions to play a role in anode passivation, but the produced molybdate can also react with rust to form complexes of heteropolyacids, thereby stabilizing the rust. In addition, the presence of molybdenum ions can increase the polarization resistance of the steel surface, reduce the critical current density required for passivation, and increase the stability of the passivation film.
[0027] Therefore, the modified mesoporous nano zinc molybdate / zinc phosphate of the present invention uses modified mesoporous nano zinc molybdate / zinc phosphate with electrochemical protection function, and at the same time, epoxy resin modified by graphene oxide is added to achieve the purpose of improving the corrosion resistance of the coating through physical and chemical synergistic anti-corrosion effects. The addition of nano silicon dioxide can improve the adhesion of the coating through inorganic-inorganic interaction, and also improve the mechanical properties of the coating.
[0028] The anti-rust and anti-corrosion coating for the electric power tower prepared by the invention improves the anti-corrosion performance of the coating through physical and chemical synergistic anti-corrosion effects. At the same time, the coating is a water-based coating, which is green and environmentally friendly, has good flexibility, impact resistance, chemical solvent resistance, weather resistance, and salt spray resistance, has good anti-rust performance, and has broad application prospects. DETAILED DESCRIPTION
[0029] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] The dispersant 104BC is Korean KS Rheorlow DW-104BC dispersant.
[0031] Polyurethane RM-8W is Rohm and Haas thickener RM8W.
[0032] Epoxy resin DEN-425 is Dow phenolic epoxy resin DEN 425.
[0033] Example 1
[0034] This embodiment provides a method for preparing an anti-rust and anti-corrosion coating for an electric power tower, comprising the following steps:
[0035] S1. Preparation of a modifier: 3 g of piceatannol and 2 g of resveratrol were stirred and mixed for 10 min to obtain a modifier;
[0036] S2. Preparation of modified waterborne polyurethane: 10 g of polytetrahydrofuran diol 2000 was added to 50 mL of acetone, heated to 55 ° C, 5 g of toluene diisocyanate was added dropwise, stirred for 1 h, 0.01 g of dibutyltin dilaurate, 1 g of dimethylolpropionic acid, 0.2 g of 1,4-butanediol and 2 g of modifier were added, and the reaction was continued with stirring for 5 h, cooled to room temperature, 0.5 g of triethylamine was added, stirred for 30 min, 30 mL of deionized water was added, emulsified for 20 min, and acetone was removed under reduced pressure to obtain a modified waterborne polyurethane;
[0037] S3. Preparation of modified graphene oxide: 1 g of graphene oxide was dissolved in 1000 mL of water, 0.3 g of dopamine hydrochloride and 0.01 g of catalyst were added, heated to 40 ° C, stirred for 2 h, and dried to obtain modified graphene oxide;
[0038] The catalyst is a Tris-HCl solution with a pH of 8.5;
[0039] S4. Preparation of modified epoxy resin emulsion: 3g polyethylene glycol 400 and 4g epoxy resin DEN-425 were mixed, 0.5g boron trifluoride ether was added, heated to 85°C, stirred for reaction for 3h, and an emulsifier was prepared. 2g emulsifier and 60g bisphenol F epoxy resin were added to 500mL water, heated to 70°C, stirred for reaction for 1h, and then 4g modified graphene oxide and 1g nano-silicon dioxide were added, stirred for reaction for 1h, and 10000r / min colloid mill was used for 1h to prepare a modified epoxy resin emulsion;
[0040] S5. Preparation of mesoporous nano zinc molybdate / zinc phosphate: 1.9 g ammonium molybdate and 1.4 g ammonium phosphate were dissolved in 200 mL water, 10 g ethanol and 0.3 g polyethylene glycol 400 were added, and the mixture was stirred for 30 min. 100 mL of a solution containing 2.6 g zinc chloride was added dropwise, and then 0.1 g polyvinyl alcohol was added. The mixture was heated to 55 ° C. and stirred for 1 h. The mixture was centrifuged, washed, and dried to obtain mesoporous nano zinc molybdate / zinc phosphate.
[0041] S6. Preparation of modified mesoporous nano zinc molybdate / zinc phosphate: 10 g of mesoporous nano zinc molybdate / zinc phosphate was added to 200 mL of ethanol, 1 g of silane coupling agent KH692 was added, the mixture was heated to 40° C., and stirred for 1 h to obtain modified mesoporous nano zinc molybdate / zinc phosphate;
[0042] S7. Preparation of anti-rust and anti-corrosion coating for power tower: stir and mix 30g modified waterborne polyurethane, 7g modified epoxy resin emulsion, 1g N,N-dimethylethanol, 0.2g dispersant 104BC, 0.1g defoamer BYK-024 and 20mL water, add 3g modified mesoporous nano zinc molybdate / zinc phosphate, 1g carbon black and 1g talcum powder, 10000r / min colloid mill for 1h, add 0.5g polyurethane RM-8W, stir for 20min, filter and obtain the anti-rust and anti-corrosion coating for power tower.
[0043] Example 2
[0044] This embodiment provides a method for preparing an anti-rust and anti-corrosion coating for an electric power tower, comprising the following steps:
[0045] S1. Preparation of a modifier: 5 g of piceatannol and 3 g of resveratrol were stirred and mixed for 10 min to obtain a modifier;
[0046] S2. Preparation of modified waterborne polyurethane: 10 g of polytetrahydrofuran diol 2000 was added to 50 mL of acetone, heated to 65 ° C, 7 g of toluene diisocyanate was added dropwise, stirred for 1 h, 0.02 g of dibutyltin dilaurate, 2 g of dimethylolpropionic acid, 0.4 g of 1,4-butanediol and 4 g of modifier were added, and the reaction was continued with stirring for 5 h, cooled to room temperature, 1.5 g of triethylamine was added, stirred for 30 min, 30 mL of deionized water was added, emulsified for 30 min, and acetone was removed under reduced pressure to obtain a modified waterborne polyurethane;
[0047] S3. Preparation of modified graphene oxide: 1 g of graphene oxide was dissolved in 1000 mL of water, 0.6 g of dopamine hydrochloride and 0.02 g of catalyst were added, heated to 50 ° C, stirred for 4 h, and dried to obtain modified graphene oxide;
[0048] The catalyst is a Tris-HCl solution with a pH of 9.5;
[0049] S4. Preparation of modified epoxy resin emulsion: 5g of polyethylene glycol 400 and 7g of epoxy resin DEN-425 were mixed, 1g of boron trifluoride ether was added, the mixture was heated to 95°C, stirred and reacted for 5h to obtain an emulsifier, 4g of the emulsifier and 80g of bisphenol A epoxy resin were added to 500mL of water, heated to 80°C, stirred and reacted for 2h, and then 7g of modified graphene oxide and 2g of nano-silicon dioxide were added, stirred and reacted for 2h, and 12000r / min colloid mill was used for 3h to obtain a modified epoxy resin emulsion;
[0050] S5. Preparation of mesoporous nano zinc molybdate / zinc phosphate: 2.0 g ammonium molybdate and 1.5 g ammonium phosphate were dissolved in 200 mL water, 15 g ethanol and 0.5 g polyethylene glycol 400 were added, and the mixture was stirred for 30 min. 100 mL of a solution containing 2.8 g zinc chloride was added dropwise, and then 0.2 g polyvinyl alcohol was added. The mixture was heated to 65 ° C. and stirred for 2 h. The mixture was centrifuged, washed, and dried to obtain mesoporous nano zinc molybdate / zinc phosphate.
[0051] S6. Preparation of modified mesoporous nano zinc molybdate / zinc phosphate: 10 g of mesoporous nano zinc molybdate / zinc phosphate was added to 200 mL of ethanol, 2 g of silane coupling agent KH702 was added, the mixture was heated to 50° C., and the mixture was stirred for 3 h to obtain modified mesoporous nano zinc molybdate / zinc phosphate;
[0052] S7. Preparation of anti-rust and anti-corrosion coating for power tower: stir and mix 40g modified waterborne polyurethane, 10g modified epoxy resin emulsion, 2g N,N-dimethylethanol, 0.4g dispersant 104BC, 0.2g defoamer BYK-024 and 40mL water, add 4g modified mesoporous nano zinc molybdate / zinc phosphate, 3g carbon black and 2g talcum powder, 12000r / min colloid mill for 1h, add 1g polyurethane RM-8W, stir for 20min, filter and obtain the anti-rust and anti-corrosion coating for power tower.
[0053] Example 3
[0054] This embodiment provides a method for preparing an anti-rust and anti-corrosion coating for an electric power tower, comprising the following steps:
[0055] S1. Preparation of a modifier: 4 g of piceatannol and 2.5 g of resveratrol were stirred and mixed for 10 min to obtain a modifier;
[0056] S2. Preparation of modified waterborne polyurethane: 10 g of polytetrahydrofuran diol 2000 was added to 50 mL of acetone, heated to 60 ° C, 6 g of toluene diisocyanate was added dropwise, stirred for 1 h, 0.015 g of dibutyltin dilaurate, 1.5 g of dimethylolpropionic acid, 0.3 g of 1,4-butanediol and 3 g of modifier were added, and the reaction was continued with stirring for 5 h, cooled to room temperature, 1 g of triethylamine was added, stirred for 30 min, 30 mL of deionized water was added, emulsified for 25 min, and acetone was removed under reduced pressure to obtain a modified waterborne polyurethane;
[0057] S3. Preparation of modified graphene oxide: 1 g of graphene oxide was dissolved in 1000 mL of water, 0.45 g of dopamine hydrochloride and 0.015 g of catalyst were added, heated to 45 ° C, stirred for 3 h, and dried to obtain modified graphene oxide;
[0058] The catalyst is a Tris-HCl solution with a pH of 9;
[0059] S4. Preparation of modified epoxy resin emulsion: 4 g of polyethylene glycol 400 and 5.5 g of epoxy resin DEN-425 were mixed, 0.7 g of boron trifluoride ether was added, the mixture was heated to 90 ° C, stirred and reacted for 4 h to obtain an emulsifier, 3 g of the emulsifier and 70 g of bisphenol A epoxy resin were added to 500 mL of water, heated to 75 ° C, stirred and reacted for 1.5 h, and then 5.5 g of modified graphene oxide and 1.5 g of nano-silica were added, stirred and reacted for 1.5 h, and 11000 r / min colloid mill was used for 2 h to obtain a modified epoxy resin emulsion;
[0060] S5. Preparation of mesoporous nano zinc molybdate / zinc phosphate: 1.96 g ammonium molybdate and 1.46 g ammonium phosphate were dissolved in 200 mL water, 12 g ethanol and 0.4 g polyethylene glycol 400 were added, and the mixture was stirred for 30 min. 100 mL of a solution containing 2.74 g zinc chloride was added dropwise, and then 0.15 g polyvinyl alcohol was added. The mixture was heated to 60 ° C. and stirred for 1.5 h. The mixture was centrifuged, washed, and dried to obtain mesoporous nano zinc molybdate / zinc phosphate.
[0061] S6. Preparation of modified mesoporous nano zinc molybdate / zinc phosphate: 10 g of mesoporous nano zinc molybdate / zinc phosphate was added to 200 mL of ethanol, 1.5 g of silane coupling agent KH550 was added, the mixture was heated to 45° C., and stirred for 2 h to obtain modified mesoporous nano zinc molybdate / zinc phosphate;
[0062] S7. Preparation of anti-rust and anti-corrosion coating for power tower: stir and mix 35g modified waterborne polyurethane, 8g modified epoxy resin emulsion, 1.5g N,N-dimethylethanol, 0.3g dispersant 104BC, 0.15g defoamer BYK-024 and 30mL water, add 3.5g modified mesoporous nano zinc molybdate / zinc phosphate, 2g carbon black and 1.5g talcum powder, 11000r / min colloid mill for 1h, add 0.7g polyurethane RM-8W, stir for 20min, filter and obtain the anti-rust and anti-corrosion coating for power tower.
[0063] Comparative Example 1
[0064] Compared with Example 3, the difference is that no modifier is added in step S2.
[0065] The details are as follows:
[0066] S2. Preparation of modified waterborne polyurethane: Add 10g of polytetrahydrofuran diol 2000 to 50mL of acetone, heat to 60°C, add 6g of toluene diisocyanate dropwise, stir and react for 1h, add 0.015g of dibutyltin dilaurate, 1.5g of dihydroxymethylpropionic acid, and 0.3g of 1,4-butanediol, continue to stir and react for 5h, cool to room temperature, add 1g of triethylamine, stir and react for 30min, add 30mL of deionized water, emulsify for 25min, remove acetone under reduced pressure, and obtain waterborne polyurethane.
[0067] Comparative Example 2
[0068] Compared with Example 3, the difference is that in step S4, the modified graphene oxide is replaced by an equal amount of graphene oxide.
[0069] The details are as follows:
[0070] S4. Preparation of modified epoxy resin emulsion: Mix 4g polyethylene glycol 400 and 5.5g epoxy resin DEN-425, add 0.7g boron trifluoride etherate, heat to 90°C, stir and react for 4h to obtain an emulsifier, add 3g emulsifier and 70g bisphenol A epoxy resin into water, heat to 75°C, stir and react for 1.5h, then add 5.5g graphene oxide and 1.5g nano-silicon dioxide, stir and react for 1.5h, and colloid mill at 11000r / min for 2h to obtain a modified epoxy resin emulsion.
[0071] Comparative Example 3
[0072] Compared with Example 3, the difference is that ammonium phosphate is not added in step S5.
[0073] The details are as follows:
[0074] S5. Preparation of mesoporous nano zinc molybdate: Dissolve 3.42g of ammonium molybdate in 200mL of water, add 12g of ethanol and 0.4g of polyethylene glycol 400, stir and mix for 30min, add 100mL of 2.74g of zinc chloride solution, then add 0.15g of polyvinyl alcohol, heat to 60°C, stir and react for 1.5h, centrifuge, wash, and dry to obtain mesoporous nano zinc molybdate.
[0075] Comparative Example 4
[0076] Compared with Example 3, the difference is that ammonium molybdate is not added in step S5.
[0077] The details are as follows:
[0078] S5. Preparation of mesoporous nano zinc phosphate: Dissolve 3.42 g of ammonium phosphate in 200 mL of water, add 12 g of ethanol and 0.4 g of polyethylene glycol 400, stir and mix for 30 min, add 100 mL of a solution containing 2.74 g of zinc chloride, and then add 0.15 g of polyvinyl alcohol, heat to 60°C, stir and react for 1.5 h, centrifuge, wash, and dry to obtain mesoporous nano zinc phosphate.
[0079] Comparative Example 5
[0080] Compared with the embodiment 3, the difference is that step S6 is not performed.
[0081] The details are as follows:
[0082] S1. Preparation of a modifier: 4 g of piceatannol and 2.5 g of resveratrol were stirred and mixed for 10 min to obtain a modifier;
[0083] S2. Preparation of modified waterborne polyurethane: 10 g of polytetrahydrofuran diol 2000 was added to 50 mL of acetone, heated to 60 ° C, 6 g of toluene diisocyanate was added dropwise, stirred for 1 h, 0.015 g of dibutyltin dilaurate, 1.5 g of dimethylolpropionic acid, 0.3 g of 1,4-butanediol and 3 g of modifier were added, and the reaction was continued with stirring for 5 h, cooled to room temperature, 1 g of triethylamine was added, stirred for 30 min, 30 mL of deionized water was added, emulsified for 25 min, and acetone was removed under reduced pressure to obtain a modified waterborne polyurethane;
[0084] S3. Preparation of modified graphene oxide: 1 g of graphene oxide was dissolved in 1000 mL of water, 0.45 g of dopamine hydrochloride and 0.015 g of catalyst were added, heated to 45 ° C, stirred for 3 h, and dried to obtain modified graphene oxide;
[0085] The catalyst is a Tris-HCl solution with a pH of 9;
[0086] S4. Preparation of modified epoxy resin emulsion: 4 g of polyethylene glycol 400 and 5.5 g of epoxy resin DEN-425 were mixed, 0.7 g of boron trifluoride ether was added, the mixture was heated to 90 ° C, stirred and reacted for 4 h to obtain an emulsifier, 3 g of the emulsifier and 70 g of bisphenol A epoxy resin were added to water, heated to 75 ° C, stirred and reacted for 1.5 h, and then 5.5 g of modified graphene oxide and 1.5 g of nano-silicon dioxide were added, stirred and reacted for 1.5 h, and 11000 r / min colloid mill was used for 2 h to obtain a modified epoxy resin emulsion;
[0087] S5. Preparation of mesoporous nano zinc molybdate / zinc phosphate: 1.96 g ammonium molybdate and 1.46 g ammonium phosphate were dissolved in 200 mL water, 12 g ethanol and 0.4 g polyethylene glycol 400 were added, and the mixture was stirred for 30 min. 100 mL of a solution containing 2.74 g zinc chloride was added dropwise, and then 0.15 g polyvinyl alcohol was added. The mixture was heated to 60 ° C. and stirred for 1.5 h. The mixture was centrifuged, washed, and dried to obtain mesoporous nano zinc molybdate / zinc phosphate.
[0088] S6. Preparation of anti-rust and anti-corrosion coating for power tower: 35g modified waterborne polyurethane, 8g modified epoxy resin emulsion, 1.5g N,N-dimethylethanol, 0.3g dispersant 104BC, 0.15g defoamer BYK-024 and 30mL water were stirred and mixed evenly, 3.5g mesoporous nano zinc molybdate / zinc phosphate, 2g carbon black and 1.5g talcum powder were added, 11000r / min colloid mill was used for 1h, 0.7g polyurethane RM-8W was added, stirred for 20min, filtered, and the anti-rust and anti-corrosion coating for power tower was obtained.
[0089] Comparative Example 6
[0090] Compared with Example 3, the difference is that no modified epoxy resin emulsion is added in step S7.
[0091] The details are as follows:
[0092] S7. Preparation of anti-rust and anti-corrosion coating for power tower: stir and mix 35g modified waterborne polyurethane, 1.5g N,N-dimethylethanol, 0.3g dispersant 104BC, 0.15g defoamer BYK-024 and 30mL water, add 3.5g modified mesoporous nano zinc molybdate / zinc phosphate, 2g carbon black and 1.5g talcum powder, 11000r / min colloid mill for 1h, add 0.7g polyurethane RM-8W, stir for 20min, filter and obtain the anti-rust and anti-corrosion coating for power tower.
[0093] Comparative Example 7
[0094] Compared with Example 3, the difference is that no modified mesoporous nano zinc molybdate / zinc phosphate is added in step S7.
[0095] The details are as follows:
[0096] S7. Preparation of anti-rust and anti-corrosion coating for power tower: stir and mix 35g modified waterborne polyurethane, 8g modified epoxy resin emulsion, 1.5g N,N-dimethylethanol, 0.3g dispersant 104BC, 0.15g defoamer BYK-024 and 30mL water, add 2g carbon black and 1.5g talcum powder, 11000r / min colloid mill for 1h, add 0.7g polyurethane RM-8W, stir for 20min, filter and obtain the anti-rust and anti-corrosion coating for power tower.
[0097] Test Example 1
[0098] The anti-rust and anti-corrosion coatings for power towers prepared in Examples 1-3 and Comparative Examples 1-7 were sprayed on the test panels according to the requirements of GB / T1727-2021. The following tests were performed:
[0099] Adhesion test: The adhesion is tested according to GB / T5210-2006 coating adhesion test method (pull-off method).
[0100] Pencil hardness test refers to GB / T6739-2006.
[0101] The water resistance test refers to GB / T1733-1993, the test temperature is 40℃, and the test time is 24h.
[0102] The results are shown in Table 1.
[0103] Table 1
[0104] Group Adhesion(grade) Pencil hardness (H) Water resistance Example 1 0 5 No bubbling, wrinkling or shedding Example 2 0 5 No bubbling, wrinkling or shedding Example 3 0 5 No bubbling, wrinkling or shedding Comparative Example 1 1 5 Coating peeling and blistering Comparative Example 2 1 4 No bubbling, wrinkling or shedding Comparative Example 3 0 4 No bubbling, wrinkling or shedding Comparative Example 4 0 4 No bubbling, wrinkling or shedding Comparative Example 5 1 4 No bubbling, wrinkling or shedding Comparative Example 6 2 4 No bubbling, wrinkling or shedding Comparative Example 7 1 3 No bubbling, wrinkling or shedding
[0105] It can be seen from the above table that the anti-rust and anti-corrosion coatings for power towers prepared in Examples 1-3 of the present invention have higher adhesion, greater hardness and better water resistance.
[0106] Test Example 2
[0107] The anti-rust and anti-corrosion coatings for power towers prepared in Examples 1-3 and Comparative Examples 1-7 were sprayed on the test panels according to the requirements of GB / T1727-2021. The following tests were performed:
[0108] Flexibility test refers to GB / T1731-2020;
[0109] The impact resistance test refers to GB / T1732-2020, the weight of the hammer is (1000±1)g, and the paint film is magnified 4 times to observe whether it is damaged. The maximum height of the hammer drop when it is not damaged is the measurement result;
[0110] The results are shown in Table 2.
[0111] Table 2
[0112] Group Flexibility(mm) Impact resistance (kg·cm) Example 1 0.8 89 Example 2 0.6 92 Example 3 0.5 95 Comparative Example 1 1.1 85 Comparative Example 2 3.6 67 Comparative Example 3 1.9 81 Comparative Example 4 2.1 78 Comparative Example 5 2.7 74 Comparative Example 6 4.7 62 Comparative Example 7 3.3 70
[0113] It can be seen from the above table that the anti-rust and anti-corrosion coatings for electric power towers prepared in Examples 1-3 of the present invention have good flexibility, impact resistance and bending properties.
[0114] Test Example 3
[0115] The anti-rust and anti-corrosion coatings for power towers prepared in Examples 1-3 and Comparative Examples 1-7 were sprayed on the test panels according to the requirements of GB / T1727-2021. The following tests were performed:
[0116] The neutral salt spray resistance test was carried out in accordance with the provisions of GB / T1771-2007 "Determination of neutral salt spray resistance of paints and varnishes" on a JD-120 (600L) salt spray tester. The mass concentration of the sodium chloride solution was (50±5) g / L and the pH was 6.5-7.0.
[0117] The acid resistance is tested according to the immersion method specified in GB / T9274-1988 "Determination of resistance of paints and varnishes to liquid media", with a sulfuric acid mass fraction of 5%. Defects are observed after immersion for 24 hours.
[0118] The organic solvent resistance test is carried out according to the manual wiping method specified in GB / T23989-2009 "Determination of Solvent Resistance of Coatings by Wiping". Wipe back and forth 25 times with a finger wrapped in absorbent cotton to observe whether it is damaged and the base material is exposed.
[0119] The results are shown in Table 3.
[0120] Table 3
[0121]
[0122] It can be seen from the above table that the anti-rust and anti-corrosion coatings for electric power towers prepared in Examples 1-3 of the present invention have good salt spray resistance, acid resistance and solvent resistance.
[0123] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing an anti-rust and anti-corrosion coating for an electric power tower, characterized in that: The polyurethane is modified with piceatannol and resveratrol to obtain a modified waterborne polyurethane, the graphene oxide is modified with polydopamine and added into epoxy resin together with nano-silicon dioxide to obtain a modified epoxy resin emulsion, and mesoporous nano zinc molybdate / zinc phosphate is prepared and the surface is modified with a silane coupling agent, and then mixed evenly with the modified waterborne polyurethane, modified epoxy resin emulsion, pH value adjuster, dispersant, defoamer, pigment, talcum powder and water, colloid milled, thickener added, stirred evenly, filtered, and the anti-rust and anti-corrosion coating for power towers was obtained.
2. The preparation method according to claim 1, characterized in that: The following steps are involved: S1. Preparation of a modifier: mixing piceatannol and resveratrol uniformly to prepare a modifier; S2. Preparation of modified waterborne polyurethane: adding polytetrahydrofuran diol to acetone, heating, adding isocyanate dropwise, stirring to react, adding a catalyst, dimethylol propionic acid, 1,4-butanediol and a modifier, continuing to stir to react, cooling to room temperature, adding triethylamine, stirring to react, adding deionized water, emulsifying, and removing acetone under reduced pressure to obtain a modified waterborne polyurethane; S3. Preparation of modified graphene oxide: dissolving graphene oxide in water, adding dopamine hydrochloride and a catalyst, heating and stirring to react, and drying to obtain modified graphene oxide; S4. Preparation of modified epoxy resin emulsion: polyethylene glycol and multifunctional epoxy resin are mixed, boron trifluoride ether is added, heated and stirred to react, and an emulsifier is prepared, the emulsifier and epoxy resin are added to water, heated and stirred to react, and then modified graphene oxide and nano-silica are added, stirred to react, and colloid milled to prepare a modified epoxy resin emulsion; S5. Preparation of mesoporous nano zinc molybdate / zinc phosphate: dissolve ammonium molybdate and ammonium phosphate in water, add ethanol and polyethylene glycol, stir and mix evenly, dropwise add zinc chloride solution, then add polyvinyl alcohol, heat and stir to react, centrifuge, wash, and dry to obtain mesoporous nano zinc molybdate / zinc phosphate; S6. Preparation of modified mesoporous nano zinc molybdate / zinc phosphate: adding mesoporous nano zinc molybdate / zinc phosphate to ethanol, adding a silane coupling agent, heating and stirring to react, to obtain modified mesoporous nano zinc molybdate / zinc phosphate; S7. Preparation of anti-rust and anti-corrosion coating for power tower: Stir and mix modified waterborne polyurethane, modified epoxy resin emulsion, pH adjuster, dispersant, defoaming agent and water evenly, add modified mesoporous nano zinc molybdate / zinc phosphate, pigment and talcum powder, colloid mill, add thickener, stir evenly, filter, and obtain the anti-rust and anti-corrosion coating for power tower.
3. The preparation method according to claim 2, characterized in that: The mass ratio of piceatannol to resveratrol in step S1 is 3-5:2-3.
4. The preparation method according to claim 2, characterized in that: The mass ratio of the polytetrahydrofuran diol, isocyanate, catalyst, dimethylol propionic acid, 1,4-butanediol, modifier and triethylamine in step S2 is 10: 5-7: 0.01-0.02: 1-2: 0.2-0.4: 2-4: 0.5-1.5, the heating temperature is 55-65° C., the isocyanate is selected from at least one of isophorone diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, hexamethylene diisocyanate and lysine diisocyanate, the catalyst is dibutyltin dilaurate or stannous octoate, and the emulsification time is 20-30 min.
5. The preparation method according to claim 2, characterized in that: In step S3, the mass ratio of graphene oxide, dopamine hydrochloride and catalyst is 10:3-6:0.1-0.2, the temperature of the heating and stirring reaction is 40-50° C., the time is 2-4 hours, and the catalyst is a Tris-HCl solution with a pH of 8.5-9.
5.
6. The preparation method according to claim 2, characterized in that: The mass ratio of polyethylene glycol, multifunctional epoxy resin and boron trifluoride ether in step S4 is 3-5:4-7:0.5-1, the multifunctional epoxy resin is epoxy resin DEN-425, the mass ratio of the emulsifier, epoxy resin, modified graphene oxide and nano-silicon dioxide is 2-4:60-80:4-7:1-2, the rotation speed of the colloid mill is 10000-12000r / min, the time is 1-3h, and the epoxy resin is bisphenol A or bisphenol F type epoxy resin.
7. The preparation method according to claim 2, characterized in that: In step S5, the mass ratio of ammonium molybdate, ammonium phosphate, ethanol, polyethylene glycol, zinc chloride and polyvinyl alcohol is 1.9-2.0:1.4-1.5:10-15:0.3-0.5:2.6-2.8:0.1-0.2, and the temperature of the heating and stirring reaction is 55-65°C and the time is 1-2h.
8. The preparation method according to claim 2, characterized in that: In step S6, the mass ratio of the mesoporous nano zinc molybdate / zinc phosphate to the silane coupling agent is 10:1-2, the silane coupling agent is selected from at least one of KH550, KH692, and KH702, and the heating and stirring reaction is performed at a temperature of 40-50° C. for 1-3 hours.
9. The preparation method according to claim 2, characterized in that: The mass ratio of the modified waterborne polyurethane, modified epoxy resin emulsion, pH regulator, dispersant, defoamer, water, modified mesoporous nano zinc molybdate / zinc phosphate, pigment, talcum powder and thickener in step S7 is 30-40:7-10:1-2:0.2-0.4:0.1-0.2:20-40:3-4:1-3:1-2:0.5-1, the pH regulator is N,N-dimethylethanol, the dispersant is 104BC, the defoamer is BYK-024, the pigment is carbon black, and the thickener is polyurethane RM-8W.
10. An anti-rust and anti-corrosion coating for electric power towers prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method of light-resistant and waterproof waterborne polyurethane paint
CN104893540A
Graphene anticorrosive paint and preparation method thereof
CN111647342A
High-solid-content water-based graphene anticorrosive paint as well as preparation method and application thereof
CN114752279A
Cited By
Wear-resistant high-resilience sealing material and preparation method thereof
CN119798875A