Stain-resistant and scratch-resistant floor paint and production process thereof
Through the design of the floor paint with three-layer structure, the use of silicon modified polyurethane acrylic resin and polytetrafluoroethylene wax powder and other components, the problem of insufficient stain-resistant and scratch-resistant performance of existing wooden floor paint is solved, and higher wear resistance is achieved , adhesion and scratch resistance.
Patent Information
- Application Number
- CN202411253909.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-12
AI Technical Summary
The surface paint film of existing wooden floors has shortcomings in terms of stain resistance and scratch resistance, which cannot meet the high requirements of users.
Stainless scratch-resistant floor paint with a three-layer structure, including the first stain-resistant scratch-resistant layer, the second stain-resistant scratch-resistant layer and the third stain-resistant scratch-resistant layer, respectively, modified polyurethane acrylic resin and polytetrafluoroethylene. Components such as wax powder and stain-resistant additives are composed of components, and are coated and cured by an ultraviolet curing machine to ensure the excellent performance of each coat of paint.
Significantly improve the stain and scratch resistance of floor paint, achieving surface wear resistance of 0.06g/100r, paint film adhesion 5B, pencil hardness 4H, Martindale scratch resistance level 1, surface stain resistance level 4 technical indicators.
Smart Images

Figure CN118931365A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a floor paint, in particular to a stain-resistant and scratch-resistant floor paint and a production process thereof. Background Art
[0002] With the development of technology and the improvement of user needs, manufacturers and users have higher and higher requirements for the stain resistance and scratch resistance of wooden floors. However, the surface paint film of existing wooden floors can only meet the technical indicators of paint film adhesion 4B, pencil hardness 2H, and surface stain resistance level 2, which cannot meet the users' pursuit of stain resistance and scratch resistance of wooden floors.
[0003] Therefore, a floor paint with better stain and scratch resistance is needed. Summary of the invention
[0004] The object of the present invention is to provide a stain-resistant and scratch-resistant floor paint and a production process thereof, which can effectively improve the stain-resistant and scratch-resistant performance of the paint film on the floor surface.
[0005] The technical solution of the present invention is a stain-resistant and scratch-resistant floor paint, comprising a first stain-resistant and scratch-resistant layer coated on the surface of the floor, wherein the first stain-resistant and scratch-resistant layer is coated with a first stain-resistant and scratch-resistant paint, and the first stain-resistant and scratch-resistant paint contains silicon-modified polyurethane acrylic resin, polytetrafluoroethylene wax powder and stain-resistant additive.
[0006] In the aforementioned stain-resistant and scratch-resistant floor paint, the first stain-resistant and scratch-resistant paint includes, by mass, 10 to 20 parts of 12-functional hardened polyurethane acrylate, 10 to 20 parts of 8-functional hardened polyurethane acrylic resin, 10 to 20 parts of silicon-modified polyurethane acrylic resin, 1 to 3 parts of defoaming agent, 1 to 32 parts of leveling agent, 20 to 40 parts of trimethylolpropane triacrylate, 1 to 3 parts of polytetrafluoroethylene wax powder, 5 to 10 parts of silicon dioxide, 4 to 8 parts of wear-resistant material, 1 to 3 parts of 4-methylbenzophenone photosensitizer, 4 to 8 parts of methyl benzoylformate photosensitizer and 4 to 8 parts of stain-resistant additive.
[0007] In the aforementioned stain-resistant and scratch-resistant floor paint, the inner side of the first stain-resistant and scratch-resistant layer is provided with a second stain-resistant and scratch-resistant layer coated with a second stain-resistant and scratch-resistant paint, and the second stain-resistant and scratch-resistant paint includes, by mass, 20 to 40 parts of 12-functional hardened polyurethane acrylic resin, 15 to 20 parts of 8-functional hardened polyurethane acrylic resin, 1 to 3 parts of defoaming agent, 1 to 3 parts of leveling agent, 20 to 40 parts of trimethylolpropane triacrylate, 1 to 3 parts of wax powder, 5 to 10 parts of silica, 4 to 8 parts of wear-resistant material, 1 to 3 parts of 4-methylbenzophenone photosensitizer, and 4 to 8 parts of methyl benzoylformate photosensitizer.
[0008] In the aforementioned stain-resistant and scratch-resistant floor paint, the inner side of the second stain-resistant and scratch-resistant layer is provided with a third stain-resistant and scratch-resistant layer coated with a third stain-resistant and scratch-resistant paint, and the third stain-resistant and scratch-resistant paint includes, by mass, 10 to 20 parts of 12-functional hardened polyurethane acrylic resin, 15 to 25 parts of 8-functional hardened polyurethane acrylic resin, 5 to 10 parts of 6-functional polyurethane acrylic resin, 1 to 3 parts of defoaming agent, 1 to 3 parts of leveling agent, 30 to 40 parts of trimethylolpropane triacrylate, 1 to 3 parts of wax powder, 5 to 10 parts of silica, 3 to 6 parts of wear-resistant material, 1 to 3 parts of 4-methylbenzophenone photosensitizer and 3 to 6 parts of methyl benzoylformate photosensitizer.
[0009] In the aforementioned stain-resistant and scratch-resistant floor paint, the coating amount of the third stain-resistant and scratch-resistant paint is 10 to 12 g / m 2 The coating amount of the second stain-resistant and scratch-resistant paint is 15 to 18 g / m 2 The coating amount of the first stain-resistant and scratch-resistant paint is 10 to 15 g / m 2 .
[0010] The production process of the aforementioned stain-resistant and scratch-resistant floor paint comprises the following steps:
[0011] a. Apply the third stain-resistant and scratch-resistant paint on the surface of the floor, and then use a UV curing machine at 150-250mJ / cm 2 The third stain-resistant and scratch-resistant paint is completely cured with the curing energy to obtain A floor paint;
[0012] b. Apply the second stain-resistant and scratch-resistant paint on the surface of floor paint A, and then use a UV curing machine at 200-300mJ / cm 2 The second stain-resistant and scratch-resistant paint is completely cured with the curing energy to obtain B floor paint;
[0013] c. Apply the first stain-resistant and scratch-resistant paint on the surface of B floor paint, and then use a UV curing machine at 650-700mJ / cm 2 The curing energy completely cures the first stain-resistant and scratch-resistant paint to obtain a finished floor paint.
[0014] In the aforementioned production process, the preparation method of the third stain-resistant and scratch-resistant paint in step a specifically comprises the following steps:
[0015] a1. The trimethylolpropane triacrylate, defoamer and leveling agent were mixed and dispersed at a speed of 1000 to 1500 RPM for 5 to 15 minutes to obtain product A1;
[0016] a2. The 12-functional hardened polyurethane acrylic resin and the 8-functional hardened polyurethane acrylic resin were added to the A1 product, and then dispersed at a speed of 1200 to 1700 RPM for 25 to 35 minutes to obtain A2 product;
[0017] a3. The 6-functional polyurethane acrylic resin, silica, wax powder and wear-resistant material were mixed and dispersed at a speed of 1200 to 1700 RPM for 15 to 25 minutes to obtain a mixture; the mixture was then added to the A2 product and dispersed at a speed of 1200 to 1700 RPM for 15 to 25 minutes to obtain A3 product;
[0018] a4. The 4-methyl benzophenone photosensitizer and methyl benzoyl formate photosensitizer were added to A3 and dispersed at a speed of 1200 to 1700 RPM for 15 to 25 minutes to obtain a third stain-resistant and scratch-resistant paint;
[0019] The fineness of the A3 product in the step a3 is not less than 20 μm, and the viscosity of the finished third stain-resistant and scratch-resistant paint in the step a4 is 1200-1600 cp.
[0020] In the aforementioned production process, the preparation method of the second stain-resistant and scratch-resistant paint in step b specifically comprises the following steps:
[0021] b1. The trimethylolpropane triacrylate, defoamer and leveling agent were mixed and dispersed at a speed of 1000 to 1500 RPM for 5 to 15 minutes to obtain B1 product;
[0022] b2. The 12-functional hardened polyurethane acrylic resin was added to the B1 product, and then dispersed at a speed of 1200 to 1700 RPM for 25 to 35 minutes to obtain B2 product;
[0023] b3. The 8-functional hardened polyurethane acrylic resin, silica, wax powder and wear-resistant material were mixed and dispersed at a speed of 1200 to 1700 RPM for 15 to 25 minutes to obtain a mixture; the mixture was then added to the B2 product and dispersed at a speed of 1200 to 1700 RPM for 15 to 25 minutes to obtain B3 product;
[0024] b4. The 4-methyl benzophenone photosensitizer and methyl benzoyl formate photosensitizer were added to B3 products and dispersed at a speed of 1200 to 1700 RPM for 15 to 25 minutes to obtain a finished product second stain-resistant and scratch-resistant paint;
[0025] The fineness of the B3 product in the step b3 is not less than 20 μm, and the viscosity of the finished second stain-resistant and scratch-resistant paint in the step b4 is 1200-1600 cp.
[0026] In the aforementioned production process, the preparation method of the first stain-resistant and scratch-resistant paint in step c specifically comprises the following steps:
[0027] c1. The trimethylolpropane triacrylate, defoamer, leveling agent and stain resistant additive were mixed and dispersed at a speed of 1000 to 1500 RPM for 5 to 15 minutes to obtain C1 product;
[0028] c2. The 12-functional hardened polyurethane acrylate and the silicon-modified polyurethane acrylic resin were added to the C1 product, and then dispersed at a speed of 1200 to 1700 RPM for 25 to 35 minutes to obtain C2 product;
[0029] c3. The 8-functional hardened polyurethane acrylic resin, silica, polytetrafluoroethylene wax powder and wear-resistant material are mixed and dispersed at a speed of 1200 to 1700 RPM for 15 to 25 minutes to obtain a mixture; the mixture is then added to the C2 product and dispersed at a speed of 1200 to 1700 RPM for 15 to 25 minutes to obtain C3 product;
[0030] c4 4-methyl benzophenone photosensitizer and methyl benzoyl formate photosensitizer were added to C3 products and dispersed at a speed of 1200 to 1700 RPM for 15 to 25 minutes to obtain the finished product first stain-resistant and scratch-resistant paint;
[0031] The fineness of the C3 product in the step c3 is not less than 20 μm, and the viscosity of the finished first stain-resistant and scratch-resistant paint in the step c4 is 1200-1600 cp.
[0032] Compared with the prior art, the present invention has the following characteristics:
[0033] (1) The present invention adds silicon-modified polyurethane acrylic resin and polytetrafluoroethylene wax powder to the floor paint, so that after compounding, the overall stain resistance and scratch resistance of the floor paint can be effectively improved; by the coordinated coating of the second stain-resistant and scratch-resistant layer and the third stain-resistant and scratch-resistant layer, the three paint layers can promote each other and further improve the stain resistance and scratch resistance of the floor paint; on this basis, by limiting the composition, ratio and coating amount of the first stain-resistant and scratch-resistant paint, the second stain-resistant and scratch-resistant paint and the third stain-resistant and scratch-resistant paint, the floor paint of the present invention can achieve the technical indicators of surface wear resistance of 0.06g / 100r, paint film adhesion of 5B, pencil hardness of 4H, Martindale scratch resistance of level 1, and surface stain resistance of level 4;
[0034] (2) By defining the preparation methods of the first stain-resistant and scratch-resistant paint, the second stain-resistant and scratch-resistant paint, and the third stain-resistant and scratch-resistant paint, the mixed preparation effect of each paint material component can be improved, thereby ensuring the composite effect of each stain-resistant and scratch-resistant layer after coating;
[0035] Therefore, the present invention can effectively improve the stain resistance and scratch resistance of the paint film on the floor surface. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 It is a schematic diagram of the structure of the present invention;
[0037] Figure 2 These are pictures of sample 1 in the experimental example before and after the wear test;
[0038] Figure 3 These are pictures of sample 2 in the experimental example before and after the wear test;
[0039] Figure 4 These are pictures of sample 3 in the experimental example before and after the wear test;
[0040] Figure 5 These are pictures of sample 4 in the experimental example before and after the wear test;
[0041] Figure 6 This is a picture of sample 1 in the experimental example after the scratch resistance test;
[0042] Figure 7 This is a picture of sample 2 in the experimental example after the scratch resistance test;
[0043] Figure 8 This is a picture of sample 3 in the experimental example after the scratch resistance test;
[0044] Fig. 9 This is a picture of sample 4 in the experimental example after the scratch resistance test;
[0045] Fig.10 This is a picture of sample 1 in the experimental example after being smeared with a marker pen;
[0046] Fig.11 This is a picture of sample 1 in the experimental example after wiping the smear marks;
[0047] Fig.12 This is the picture of sample 3 in the experimental example after being smeared with a marker pen;
[0048] Fig.13 This is a picture of sample three in the experimental example after wiping off the smear marks.
[0049] The markings in the attached drawings are: 1-the first stain-resistant and scratch-resistant layer, 2-the second stain-resistant and scratch-resistant layer, 3-the third stain-resistant and scratch-resistant layer. DETAILED DESCRIPTION
[0050] The present invention is further described below in conjunction with the accompanying drawings and embodiments, but they are not intended to limit the present invention.
[0051] Example 1. A stain-resistant and scratch-resistant floor paint, comprising: Figure 1 As shown, it includes a first stain-resistant and scratch-resistant layer 1 coated on the surface of the floor, wherein the first stain-resistant and scratch-resistant layer 1 is coated with a first stain-resistant and scratch-resistant paint, wherein the first stain-resistant and scratch-resistant paint contains silicon-modified polyurethane acrylic resin, polytetrafluoroethylene wax powder and stain-resistant additive.
[0052] The first stain-resistant and scratch-resistant paint includes, by mass, 10 to 20 parts of 12-functional hardened polyurethane acrylate, 10 to 20 parts of 8-functional hardened polyurethane acrylic resin, 10 to 20 parts of silicon-modified polyurethane acrylic resin, 1 to 3 parts of defoaming agent, 1 to 32 parts of leveling agent, 20 to 40 parts of trimethylolpropane triacrylate, 1 to 3 parts of polytetrafluoroethylene wax powder, 5 to 10 parts of silicon dioxide, 4 to 8 parts of wear-resistant material, 1 to 3 parts of 4-methylbenzophenone photosensitizer, 4 to 8 parts of methyl benzoylformate photosensitizer and 4 to 8 parts of stain-resistant additive.
[0053] The inner side of the first stain-resistant and scratch-resistant layer 1 is provided with a second stain-resistant and scratch-resistant layer 2 coated with a second stain-resistant and scratch-resistant paint, and the second stain-resistant and scratch-resistant paint includes, by mass, 20 to 40 parts of 12-functional hardened polyurethane acrylic resin, 15 to 20 parts of 8-functional hardened polyurethane acrylic resin, 1 to 3 parts of defoaming agent, 1 to 3 parts of leveling agent, 20 to 40 parts of trimethylolpropane triacrylate, 1 to 3 parts of wax powder, 5 to 10 parts of silica, 4 to 8 parts of wear-resistant material, 1 to 3 parts of 4-methylbenzophenone photosensitizer, and 4 to 8 parts of methyl benzoylformate photosensitizer.
[0054] The inner side of the second stain-resistant and scratch-resistant layer 2 is provided with a third stain-resistant and scratch-resistant layer 3 coated with a third stain-resistant and scratch-resistant paint, and the third stain-resistant and scratch-resistant paint includes, by mass, 10 to 20 parts of 12-functional hardened polyurethane acrylic resin, 15 to 25 parts of 8-functional hardened polyurethane acrylic resin, 5 to 10 parts of 6-functional polyurethane acrylic resin, 1 to 3 parts of defoaming agent, 1 to 3 parts of leveling agent, 30 to 40 parts of trimethylolpropane triacrylate, 1 to 3 parts of wax powder, 5 to 10 parts of silica, 3 to 6 parts of wear-resistant material, 1 to 3 parts of 4-methylbenzophenone photosensitizer and 3 to 6 parts of methyl benzoylformate photosensitizer.
[0055] The wax powder is polyethylene wax powder.
[0056] The coating amount of the third stain-resistant and scratch-resistant paint is 10 to 12 g / m 2 The coating amount of the second stain-resistant and scratch-resistant paint is 15 to 18 g / m 2 The coating amount of the first stain-resistant and scratch-resistant paint is 10 to 15 g / m 2 .
[0057] The production process of the stain-resistant and scratch-resistant floor paint comprises the following steps:
[0058] a. Apply the third stain-resistant and scratch-resistant paint on the surface of the floor, and then use a UV curing machine at 150-250mJ / cm 2 The third stain-resistant and scratch-resistant paint is completely cured with the curing energy to obtain A floor paint;
[0059] b. Apply the second stain-resistant and scratch-resistant paint on the surface of floor paint A, and then use a UV curing machine at 200-300mJ / cm 2 The second stain-resistant and scratch-resistant paint is completely cured with the curing energy to obtain B floor paint;
[0060] c. Apply the first stain-resistant and scratch-resistant paint on the surface of B floor paint, and then use a UV curing machine at 650-700mJ / cm 2 The curing energy completely cures the first stain-resistant and scratch-resistant paint to obtain a finished floor paint.
[0061] The preparation method of the third stain-resistant and scratch-resistant paint in step a specifically comprises the following steps:
[0062] a1. The trimethylolpropane triacrylate, defoamer and leveling agent were mixed and dispersed at a speed of 1000 to 1500 RPM for 5 to 15 minutes to obtain product A1;
[0063] a2. The 12-functional hardened polyurethane acrylic resin and the 8-functional hardened polyurethane acrylic resin were added to the A1 product, and then dispersed at a speed of 1200 to 1700 RPM for 25 to 35 minutes to obtain A2 product;
[0064] a3. The 6-functional polyurethane acrylic resin, silica, wax powder and wear-resistant material were mixed and dispersed at a speed of 1200 to 1700 RPM for 15 to 25 minutes to obtain a mixture; the mixture was then added to the A2 product and dispersed at a speed of 1200 to 1700 RPM for 15 to 25 minutes to obtain A3 product;
[0065] a4. The 4-methyl benzophenone photosensitizer and methyl benzoyl formate photosensitizer were added to A3 and dispersed at a speed of 1200 to 1700 RPM for 15 to 25 minutes to obtain a third stain-resistant and scratch-resistant paint;
[0066] The fineness of the A3 product in the step a3 is not less than 20 μm, and the viscosity of the finished third stain-resistant and scratch-resistant paint in the step a4 is 1200-1600 cp.
[0067] The preparation method of the second stain-resistant and scratch-resistant paint in step b specifically comprises the following steps:
[0068] b1. The trimethylolpropane triacrylate, defoamer and leveling agent were mixed and dispersed at a speed of 1000 to 1500 RPM for 5 to 15 minutes to obtain B1 product;
[0069] b2. The 12-functional hardened polyurethane acrylic resin was added to the B1 product, and then dispersed at a speed of 1200 to 1700 RPM for 25 to 35 minutes to obtain B2 product;
[0070] b3. The 8-functional hardened polyurethane acrylic resin, silica, wax powder and wear-resistant material were mixed and dispersed at a speed of 1200 to 1700 RPM for 15 to 25 minutes to obtain a mixture; the mixture was then added to the B2 product and dispersed at a speed of 1200 to 1700 RPM for 15 to 25 minutes to obtain B3 product;
[0071] b4. The 4-methyl benzophenone photosensitizer and methyl benzoyl formate photosensitizer were added to B3 products and dispersed at a speed of 1200 to 1700 RPM for 15 to 25 minutes to obtain a finished product second stain-resistant and scratch-resistant paint;
[0072] The fineness of the B3 product in the step b3 is not less than 20 μm, and the viscosity of the finished second stain-resistant and scratch-resistant paint in the step b4 is 1200-1600 cp.
[0073] The method for preparing the first stain-resistant and scratch-resistant paint in step c specifically comprises the following steps:
[0074] c1. The trimethylolpropane triacrylate, defoamer, leveling agent and stain resistant additive were mixed and dispersed at a speed of 1000 to 1500 RPM for 5 to 15 minutes to obtain C1 product;
[0075] c2. The 12-functional hardened polyurethane acrylate and the silicon-modified polyurethane acrylic resin were added to the C1 product, and then dispersed at a speed of 1200 to 1700 RPM for 25 to 35 minutes to obtain C2 product;
[0076] c3. The 8-functional hardened polyurethane acrylic resin, silica, polytetrafluoroethylene wax powder and wear-resistant material are mixed and dispersed at a speed of 1200 to 1700 RPM for 15 to 25 minutes to obtain a mixture; the mixture is then added to the C2 product and dispersed at a speed of 1200 to 1700 RPM for 15 to 25 minutes to obtain C3 product;
[0077] c4 4-methyl benzophenone photosensitizer and methyl benzoyl formate photosensitizer were added to C3 products and dispersed at a speed of 1200 to 1700 RPM for 15 to 25 minutes to obtain the finished product first stain-resistant and scratch-resistant paint;
[0078] The fineness of the C3 product in the step c3 is not less than 20 μm, and the viscosity of the finished first stain-resistant and scratch-resistant paint in the step c4 is 1200-1600 cp.
[0079] This embodiment adds silicon-modified polyurethane acrylic resin and polytetrafluoroethylene wax powder to the floor paint so that they can cooperate with other components in the first stain-resistant and scratch-resistant paint, thereby improving the stain-resistant and scratch-resistant performance of the floor paint after coating.
[0080] Example 2. A stain-resistant and scratch-resistant floor paint, comprising: Figure 1As shown, it includes a first stain-resistant and scratch-resistant layer 1 coated on the surface of the floor, wherein the first stain-resistant and scratch-resistant layer 1 is coated with a first stain-resistant and scratch-resistant paint, wherein the first stain-resistant and scratch-resistant paint contains silicon-modified polyurethane acrylic resin, polytetrafluoroethylene wax powder and stain-resistant additive.
[0081] The first stain-resistant and scratch-resistant paint includes, by mass, 15 parts of 12-functional hardened polyurethane acrylate, 12 parts of 8-functional hardened polyurethane acrylic resin, 15 parts of silicon-modified polyurethane acrylic resin, 1 part of defoaming agent, 2 parts of leveling agent, 30 parts of trimethylolpropane triacrylate, 1.4 parts of polytetrafluoroethylene wax powder, 7 parts of silica, 5 parts of wear-resistant materials, 2 parts of 4-methylbenzophenone photosensitizer, 5 parts of methyl benzoylformate photosensitizer and 5 parts of stain-resistant additive.
[0082] The inner side of the first stain-resistant and scratch-resistant layer 1 is provided with a second stain-resistant and scratch-resistant layer 2 coated with a second stain-resistant and scratch-resistant paint, and the second stain-resistant and scratch-resistant paint includes, by mass, 30 parts of 12-functional hardened polyurethane acrylic resin, 17 parts of 8-functional hardened polyurethane acrylic resin, 1 part of defoaming agent, 2 parts of leveling agent, 30 parts of trimethylolpropane triacrylate, 1.4 parts of wax powder, 7 parts of silica, 5 parts of wear-resistant material, 2 parts of 4-methylbenzophenone photosensitizer, and 5 parts of methyl benzoylformate photosensitizer.
[0083] The inner side of the second stain-resistant and scratch-resistant layer 2 is provided with a third stain-resistant and scratch-resistant layer 3 coated with a third stain-resistant and scratch-resistant paint, and the third stain-resistant and scratch-resistant paint includes, by mass, 15 parts of 12-functional hardened polyurethane acrylic resin, 20 parts of 8-functional hardened polyurethane acrylic resin, 7 parts of 6-functional polyurethane acrylic resin, 1 part of defoaming agent, 2 parts of leveling agent, 35 parts of trimethylolpropane triacrylate, 1.4 parts of wax powder, 7 parts of silica, 5 parts of wear-resistant material, 2 parts of 4-methylbenzophenone photosensitizer and 5 parts of methyl benzoylformate photosensitizer.
[0084] The coating amount of the third stain-resistant and scratch-resistant paint is 10 g / m 2 The coating amount of the second stain-resistant and scratch-resistant paint is 15g / m 2 The coating amount of the first stain-resistant and scratch-resistant paint is 10 g / m 2 .
[0085] The production process of the stain-resistant and scratch-resistant floor paint comprises the following steps:
[0086] a. Apply the third stain-resistant and scratch-resistant paint on the surface of the floor, and then use a UV curing machine at 200mJ / cm 2 The third stain-resistant and scratch-resistant paint is completely cured with the curing energy to obtain A floor paint;
[0087] b. Apply a second stain-resistant and scratch-resistant paint on the surface of floor paint A, and then use a UV curing machine at 260mJ / cm2 The second stain-resistant and scratch-resistant paint is completely cured with the curing energy to obtain B floor paint;
[0088] c. Apply the first stain-resistant and scratch-resistant paint on the surface of B floor paint, and then use a UV curing machine at 680mJ / cm 2 The curing energy completely cures the first stain-resistant and scratch-resistant paint to obtain a finished floor paint.
[0089] The preparation method of the third stain-resistant and scratch-resistant paint in step a specifically comprises the following steps:
[0090] a1. The trimethylolpropane triacrylate, defoamer and leveling agent were mixed and dispersed at a speed of 1200RPM for 10 minutes to obtain A1 product;
[0091] a2. The 12-functional hardened polyurethane acrylic resin and the 8-functional hardened polyurethane acrylic resin were added to the A1 product, and then dispersed at a speed of 1500RPM for 30 minutes to obtain A2 product;
[0092] a3. The 6-functional polyurethane acrylic resin, silica, wax powder and wear-resistant material were mixed and dispersed at a speed of 1500RPM for 20 minutes to obtain a mixture; the mixture was then added to the A2 product and dispersed at a speed of 1500RPM for 20 minutes to obtain A3 product;
[0093] a4 4-methyl benzophenone photosensitizer and methyl benzoyl formate photosensitizer were added to A3 products and dispersed at a speed of 1500RPM for 20 minutes to obtain a third stain-resistant and scratch-resistant paint;
[0094] The preparation method of the second stain-resistant and scratch-resistant paint in step b specifically comprises the following steps:
[0095] b1. The trimethylolpropane triacrylate, defoamer and mixture were dispersed at a speed of 1000 to 1200 RPM for 10 minutes to obtain B1 product;
[0096] b2. The 12-functional hardened polyurethane acrylic resin was added to the B1 product, and then dispersed at a speed of 1500RPM for 30 minutes to obtain B2 product;
[0097] b3. The 8-functional hardened polyurethane acrylic resin, silica, wax powder and wear-resistant material were mixed and dispersed at a speed of 1500RPM for 20 minutes to obtain a mixture; the mixture was then added to the B2 product and dispersed at a speed of 1500RPM for 20 minutes to obtain B3 product;
[0098] b4 4-methyl benzophenone photosensitizer and methyl benzoyl formate photosensitizer was added to B3 product and dispersed at a speed of 1500RPM for 20 minutes to obtain the finished product second stain-resistant and scratch-resistant paint;
[0099] The method for preparing the first stain-resistant and scratch-resistant paint in step c specifically comprises the following steps:
[0100] c1 trimethylolpropane triacrylate, defoamer, leveling agent and stain resistant additive were mixed and dispersed at a speed of 1200RPM for 10 minutes to obtain C1 product;
[0101] c2. The 12-functional hardened polyurethane acrylate and silicon-modified polyurethane acrylic resin were added to the C1 product, and then dispersed at a speed of 1500RPM for 30 minutes to obtain C2 product;
[0102] c3 8 functional group hardened polyurethane acrylic resin, silica, polytetrafluoroethylene wax powder and wear-resistant material were mixed and dispersed at a speed of 1500RPM for 20 minutes to obtain a mixture; the mixture was then added to C2 product and dispersed at a speed of 1500RPM for 20 minutes to obtain C3 product;
[0103] c4 4-methyl benzophenone photosensitizer and methyl benzoyl formate photosensitizer was added to C3 products and dispersed at a speed of 1500RPM for 20 minutes to obtain the finished product first stain-resistant and scratch-resistant paint;
[0104] Compared with Example 1, this example further limits the composition, ratio and coating amount of the first stain-resistant and scratch-resistant paint, the second stain-resistant and scratch-resistant paint and the third stain-resistant and scratch-resistant paint, and accordingly optimizes the preparation method of each stain-resistant and scratch-resistant paint, so that it can further improve the stain-resistant and scratch-resistant performance of the floor paint after molding.
[0105] Experimental example: The nanoemulsion prepared in Example 2 is used as sample one, and three groups of floor paints prepared from different first stain-resistant and scratch-resistant paint components are set as comparative examples to obtain samples two to four respectively. The components of the first stain-resistant and scratch-resistant paint in samples two to four are shown in Table 1. Compared with Example 2, the first stain-resistant and scratch-resistant paint component of sample two removes the silicon-modified polyurethane acrylic resin. Compared with Example 2, the first stain-resistant and scratch-resistant paint component of sample three replaces the polytetrafluoroethylene wax powder with polyethylene wax powder. Compared with Example 2, the first stain-resistant and scratch-resistant paint component of sample four removes both the silicon-modified polyurethane acrylic resin and the polytetrafluoroethylene wax powder. The other components and proportions in the first stain-resistant and scratch-resistant paint are the same as those in Example 2; and the second stain-resistant and scratch-resistant layer and the third stain-resistant and scratch-resistant layer in samples two to four are the same as those in Example 2.
[0106] Table 1: Composition of the first stain-resistant and scratch-resistant paint in the four groups of samples
[0107] Group Silicon modified polyurethane acrylic resin Wax powder Sample 1 √ PTFE wax powder Sample 2 / PTFE wax powder Sample 3 √ Polyethylene wax powder Sample 4 / /
[0108] The surface wear resistance of the four groups of samples was tested according to the paint film surface wear resistance test method of GB / T18103-2022, the paint film adhesion of the four groups of samples was tested according to the test method of ASTM D335, the pencil hardness of the four groups of samples was tested according to the pencil hardness test method, the scratch resistance of the four groups of samples was tested by Martindale abrasion tester, and the surface stain resistance of the four groups of samples was tested according to the surface stain resistance test method of GB / T18103-2022. The test results are shown in Table 2:
[0109] Table 2: Test results of four groups of samples
[0110]
[0111]
[0112] Sample 1 before and after the surface wear test Figure 2 As shown (the left picture is before the test, the back picture is after the test), the mass of sample 1 before the wear test is 120.819g, the mass after the wear test is 120.755g, and the wear value is 0.06g / 100r.
[0113] Sample 2 before and after the surface wear test Figure 3 As shown (the left picture is before the test, the back picture is after the test), the mass of sample 1 before the wear test is 114.675g, the mass after the wear test is 114.564g, and the wear value is 0.11g / 100r.
[0114] Sample 3 before and after the surface wear test Figure 4 As shown (the left picture is before the test, the back picture is after the test), the mass of sample 1 before the wear test is 120.069g, the mass after the wear test is 119.982g, and the wear value is 0.09g / 100r.
[0115] Sample 4 before and after the surface wear test Figure 5 As shown (the left picture is before the test, the back picture is after the test), the mass of sample 1 before the wear test is 120.278 gg, the mass after the wear test is 120.137 gg, and the wear value is 0.14 g / 100 r.
[0116] By comparison, it can be seen that the wear resistance of sample one is better than that of sample three, and the wear resistance of sample two and sample four is lower than that of sample three, indicating that the present application can effectively improve the wear resistance of floor paint after coating by combining silicon-modified polyurethane acrylic resin and polytetrafluoroethylene wax powder.
[0117] The test standards of the Martindale abrasion tester are level 1: no visible scratches, level 2: a few scratches and no continuous pattern, level 3: a lot of scratches and slight continuous pattern, level 4: a lot of scratches and continuous scratches, and level 5: the surface is worn out and covered with micro scratches. The pictures of samples 1 to 4 after the scratch resistance test are as follows: Figure 6-9 As shown in the picture, it can be seen that the surface of sample one has no visible scratches, the surface of sample three has a large number of continuous slight scratches, and the surfaces of samples two and four are completely blurred without clear continuous scratches, indicating that the sample of Example 2 can effectively improve the scratch resistance of the floor paint after coating compared with other samples.
[0118] The paint film surfaces of sample 1 and sample 3 were smeared with a black marker pen, and then the smear marks were wiped off with a wet towel. The pictures of the two samples after smearing and wiping are as follows: Figure 10-13 As shown, Fig.10 and Fig.12 These are the state diagrams of sample 1 and sample 3 after being smeared with a marker pen. Fig.11 and Fig.13 These are the status diagrams of sample one and sample three after wiping the smear marks with water. By comparison, it can be seen that sample one did not form obvious smear marks after being smeared with a marker pen, and the towel was able to completely wipe off the ink floating on the surface of the paint film after wiping. However, sample three formed obvious smear marks after being smeared with a marker pen, and it could not be wiped off with a towel. This shows that the present application can form a special promotion effect after mixing silicon-modified polyurethane acrylic resin, polytetrafluoroethylene wax powder and other first stain-resistant and scratch-resistant paint components, which greatly improves the stain resistance of the floor paint after coating.
Claims
1. A stain-resistant and scratch-resistant floor paint, characterized in that: It comprises a first stain-resistant and scratch-resistant layer (1) coated on the surface of the floor, wherein the first stain-resistant and scratch-resistant layer (1) is formed by coating a first stain-resistant and scratch-resistant paint, wherein the first stain-resistant and scratch-resistant paint contains silicon-modified polyurethane acrylic resin, polytetrafluoroethylene wax powder and stain-resistant additive.
2. The stain-resistant and scratch-resistant floor paint according to claim 1, characterized in that: The first stain-resistant and scratch-resistant paint includes, by mass, 10 to 20 parts of 12-functional hardened polyurethane acrylate, 10 to 20 parts of 8-functional hardened polyurethane acrylic resin, 10 to 20 parts of silicon-modified polyurethane acrylic resin, 1 to 3 parts of defoaming agent, 1 to 32 parts of leveling agent, 20 to 40 parts of trimethylolpropane triacrylate, 1 to 3 parts of polytetrafluoroethylene wax powder, 5 to 10 parts of silicon dioxide, 4 to 8 parts of wear-resistant material, 1 to 3 parts of 4-methylbenzophenone photosensitizer, 4 to 8 parts of methyl benzoylformate photosensitizer and 4 to 8 parts of stain-resistant additive.
3. The stain-resistant and scratch-resistant floor paint according to claim 1, characterized in that: The inner side of the first stain-resistant and scratch-resistant layer (1) is provided with a second stain-resistant and scratch-resistant layer (2) coated with a second stain-resistant and scratch-resistant paint, wherein the second stain-resistant and scratch-resistant paint comprises, by weight, 20 to 40 parts of a 12-functional hardened polyurethane acrylic resin, 15 to 20 parts of an 8-functional hardened polyurethane acrylic resin, 1 to 3 parts of a defoaming agent, 1 to 3 parts of a leveling agent, 20 to 40 parts of trimethylolpropane triacrylate, 1 to 3 parts of wax powder, 5 to 10 parts of silicon dioxide, 4 to 8 parts of a wear-resistant material, 1 to 3 parts of 4-methylbenzophenone photosensitizer, and 4 to 8 parts of methyl benzoylformate photosensitizer.
4. The stain-resistant and scratch-resistant floor paint according to claim 3, characterized in that: The inner side of the second stain-resistant and scratch-resistant layer (2) is provided with a third stain-resistant and scratch-resistant layer (3) coated with a third stain-resistant and scratch-resistant paint, wherein the third stain-resistant and scratch-resistant paint comprises, by weight, 10 to 20 parts of a 12-functional hardened polyurethane acrylic resin, 15 to 25 parts of an 8-functional hardened polyurethane acrylic resin, 5 to 10 parts of a 6-functional polyurethane acrylic resin, 1 to 3 parts of a defoaming agent, 1 to 3 parts of a leveling agent, 30 to 40 parts of trimethylolpropane triacrylate, 1 to 3 parts of wax powder, 5 to 10 parts of silicon dioxide, 3 to 6 parts of a wear-resistant material, 1 to 3 parts of a 4-methylbenzophenone photosensitizer, and 3 to 6 parts of a methyl benzoylformate photosensitizer.
5. The stain-resistant and scratch-resistant floor paint according to claim 4, characterized in that: The coating amount of the third stain-resistant and scratch-resistant paint is 10 to 12 g / m 2 The coating amount of the second stain-resistant and scratch-resistant paint is 15 to 18 g / m 2 The coating amount of the first stain-resistant and scratch-resistant paint is 10 to 15 g / m 2 .
6. A production process for a stain-resistant and scratch-resistant floor paint according to any one of claims 1 to 5, characterized in that: The following steps are involved: a. Apply the third stain-resistant and scratch-resistant paint on the surface of the floor, and then use a UV curing machine at 150-250mJ / cm 2 The third stain-resistant and scratch-resistant paint is completely cured with the curing energy to obtain A floor paint; b. Apply the second stain-resistant and scratch-resistant paint on the surface of floor paint A, and then use a UV curing machine at 200-300mJ / cm 2 The second stain-resistant and scratch-resistant paint is completely cured with the curing energy to obtain B floor paint; c. Apply the first stain-resistant and scratch-resistant paint on the surface of B floor paint, and then use a UV curing machine at 650-700mJ / cm 2 The curing energy completely cures the first stain-resistant and scratch-resistant paint to obtain a finished floor paint.
7. The production process according to claim 6, characterized in that: The preparation method of the third stain-resistant and scratch-resistant paint in step a specifically comprises the following steps: a1. The trimethylolpropane triacrylate, defoamer and leveling agent were mixed and dispersed at a speed of 1000 to 1500 RPM for 5 to 15 minutes to obtain product A1; a2. The 12-functional hardened polyurethane acrylic resin and the 8-functional hardened polyurethane acrylic resin were added to the A1 product, and then dispersed at a speed of 1200 to 1700 RPM for 25 to 35 minutes to obtain A2 product; a3. The 6-functional polyurethane acrylic resin, silica, wax powder and wear-resistant material were mixed and dispersed at a speed of 1200 to 1700 RPM for 15 to 25 minutes to obtain a mixture; the mixture was then added to the A2 product and dispersed at a speed of 1200 to 1700 RPM for 15 to 25 minutes to obtain A3 product; a4. The 4-methyl benzophenone photosensitizer and methyl benzoyl formate photosensitizer were added to A3 and dispersed at a speed of 1200 to 1700 RPM for 15 to 25 minutes to obtain a third stain-resistant and scratch-resistant paint; The fineness of the A3 product in the step a3 is not less than 20 μm, and the viscosity of the finished third stain-resistant and scratch-resistant paint in the step a4 is 1200-1600 cp.
8. The production process according to claim 6, characterized in that: The preparation method of the second stain-resistant and scratch-resistant paint in step b specifically comprises the following steps: b1. The trimethylolpropane triacrylate, defoamer and leveling agent were mixed and dispersed at a speed of 1000 to 1500 RPM for 5 to 15 minutes to obtain B1 product; b2. The 12-functional hardened polyurethane acrylic resin was added to the B1 product, and then dispersed at a speed of 1200 to 1700 RPM for 25 to 35 minutes to obtain B2 product; b3. The 8-functional hardened polyurethane acrylic resin, silica, wax powder and wear-resistant material were mixed and dispersed at a speed of 1200 to 1700 RPM for 15 to 25 minutes to obtain a mixture; the mixture was then added to the B2 product and dispersed at a speed of 1200 to 1700 RPM for 15 to 25 minutes to obtain B3 product; b4. The 4-methyl benzophenone photosensitizer and methyl benzoyl formate photosensitizer were added to B3 products and dispersed at a speed of 1200 to 1700 RPM for 15 to 25 minutes to obtain a finished product second stain-resistant and scratch-resistant paint; The fineness of the B3 product in the step b3 is not less than 20 μm, and the viscosity of the finished second stain-resistant and scratch-resistant paint in the step b4 is 1200-1600 cp.
9. The production process according to claim 6, characterized in that: The method for preparing the first stain-resistant and scratch-resistant paint in step c specifically comprises the following steps: c1. The trimethylolpropane triacrylate, defoamer, leveling agent and stain resistant additive were mixed and dispersed at a speed of 1000 to 1500 RPM for 5 to 15 minutes to obtain C1 product; c2. The 12-functional hardened polyurethane acrylate and the silicon-modified polyurethane acrylic resin were added to the C1 product, and then dispersed at a speed of 1200 to 1700 RPM for 25 to 35 minutes to obtain C2 product; c3. The 8-functional hardened polyurethane acrylic resin, silica, polytetrafluoroethylene wax powder and wear-resistant material are mixed and dispersed at a speed of 1200 to 1700 RPM for 15 to 25 minutes to obtain a mixture; the mixture is then added to the C2 product and dispersed at a speed of 1200 to 1700 RPM for 15 to 25 minutes to obtain C3 product; c4 4-methyl benzophenone photosensitizer and methyl benzoyl formate photosensitizer were added to C3 products and dispersed at a speed of 1200 to 1700 RPM for 15 to 25 minutes to obtain the finished product first stain-resistant and scratch-resistant paint; The fineness of the C3 product in the step c3 is not less than 20 μm, and the viscosity of the finished first stain-resistant and scratch-resistant paint in the step c4 is 1200-1600 cp.
Citation Information
Patent Citations
High-wear-resistance antiscratch and antifouling solid wood board ultraviolet (UV) curable coating system
CN102190938A
Ultraviolet cured high-anti-fouling matte floor paint and preparation method thereof
CN108913012A
Multifunctional finishing paint for SPC floor
CN114350246A
Wear-resistant and stain-resistant UV (ultraviolet) hand feeling coating as well as preparation method and application thereof
CN115584199A
Wear-resistant, anti-slip and antibacterial floor ultraviolet curing coating system
CN115717021A