Novel organic silicon-niobium carbide high-temperature-resistant heavy anti-corrosion coating and preparation method thereof
Through the new silicone-niobium carbide high-temperature heavy corrosion-resistant coating, the problem of existing coatings easy to decompose in high-temperature acidic/alkaline environments is solved, and efficient corrosion resistance is provided. It is suitable for cement clinker production lines and the cement kiln is realized. Long-term anti-corrosion of the equipment.
Patent Information
- Application Number
- CN202411195776.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-12
AI Technical Summary
The existing silicone anticorrosion coatings are easy to decompose in high-temperature acidic/alkaline environments, have poor adhesion and low mechanical strength, and cannot effectively prevent corrosion of the equipment under the new operating conditions of cement clinker production lines.
The new silicone-niobium carbide high-temperature heavy corrosion-resistant coating is used, and the composition includes materials such as silicone resin, niobium carbide, etc. It forms high-performance coatings through specific formulations and preparation processes, which can provide long-term corrosion protection in high-temperature environments.
It significantly improves the wear resistance, thermal shock and corrosion resistance of the coating, is suitable for cement clinker production lines, fills the gap in the long-term use of anticorrosion materials in China, and achieves efficient corrosion protection for cement kiln equipment.
Smart Images

Figure CN118931380A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of production and preparation of anticorrosive coatings for cement production line equipment and coating construction, and in particular to a novel organosilicon-niobium carbide high temperature resistant heavy anticorrosive coating and a preparation technology thereof. Background Art
[0002] In order to achieve the new "dual carbon" goal, develop new low-carbon cement production technology, and realize energy conservation and emission reduction in the cement industry, the key is to achieve low-carbon and energy-saving production in the cement clinker production process. However, the "low-carbon production" upgrade and "pollution reduction" transformation of the cement kiln clinker production line will inevitably lead to great changes in the actual operating conditions. The final result is that it will directly or indirectly cause different types and degrees of corrosion of the structural components in various links of the production line. Traditional cement clinker production lines usually use ceramic patches, clay and other measures to achieve corrosion protection for production equipment. Due to changes in working conditions, the existing solutions are no longer sufficient to achieve effective corrosion protection under new working conditions.
[0003] A large number of practices have proved that organic silicon anti-corrosion coatings have properties such as high temperature resistance and corrosion resistance, and are expected to adapt to the new working conditions of new cement clinker production lines to achieve effective anti-corrosion. However, the organic silicon anti-corrosion coatings on the market are very easy to decompose in high-temperature acidic and high-temperature alkaline environments, have poor adhesion to the substrate, low mechanical strength, and a very short service life in high-temperature acidic / alkaline environments.
[0004] Therefore, developing a new type of anti-corrosion coating that can adapt to the new working conditions of cement clinker production lines is an urgent problem to be solved.
[0005] Niobium carbide has excellent properties such as high melting point (3500℃), high hardness (microhardness>235GPa, harder than corundum), good chemical stability, etc. It is insoluble in cold or hot hydrochloric acid, sulfuric acid, and nitric acid, and has high thermal conductivity. As an additive, it can significantly improve the material's wear resistance, thermal shock resistance, and corrosion resistance. Summary of the invention
[0006] The purpose of the present invention is to solve the problems of the above-mentioned prior art, to solve the problems of long-term heat resistance and corrosion protection of metal substrates of production lines in high temperature (temperature ≥ 400°C) acidic gas environments in the cement industry, and to provide a new type of organosilicon-niobium carbide high temperature resistant heavy anti-corrosion coating and its preparation technology.
[0007] The technical solution adopted by the present invention to solve the technical problem is: a new type of organosilicon-niobium carbide high temperature resistant heavy anti-corrosion coating and its preparation method, the coating is composed of two components A and B, the component A is composed of organosilicon resin, co-solvent, graphene powder, carbon nanofiber, graphite powder, nano zinc oxide, nano titanium oxide, silicon carbide, niobium carbide, boron nitride, zinc powder / aluminum powder, dispersant, defoamer, anti-flash rust additive and drying agent, and the component B is composed of co-solvent and curing agent. The specific coating formula is as follows by weight:
[0008] Component A: organic silicon resin: 10-45wt.%, cosolvent: 5-20wt.%, graphene powder: 0.1-2wt.%, carbon fiber powder: 0.1-2wt.%, graphite powder: 1-5wt.%, nano titanium oxide: 1-10wt.%, nano zinc oxide: 1-10wt.%, silicon carbide: 1-10wt.%, niobium carbide: 1-10wt.%, boron nitride: 1-10wt.%, zinc powder / aluminum powder: 5-20wt.%, mica powder: 1-10wt.%, low melting point filler: 5-30wt.%, dispersant: 0.2-3wt.%, defoamer: 0.2-3wt.%, anti-flash rust additive: 0.2-3wt.%, leveling agent: 0.2-3wt.%;
[0009] Component B: cosolvent: 5-15wt.%, curing agent: 5-15wt.%;
[0010] Add component B to component A and cure at room temperature to 80°C for 2-10 hours to prepare a new type of organosilicon-niobium carbide high temperature resistant heavy anti-corrosion coating.
[0011] The silicone resin is one or more of pure silicone resin (polysilazane or polysiloxane), methyl silicone resin, methylphenyl silicone resin, silicone polyester resin, silicone alkyd resin, silicone acrylic resin and silicone epoxy resin.
[0012] The co-solvent is one or more of methanol, ethanol, toluene, xylene, trimethylbenzene, n-butanol, 1,4-butanediol, acetone, isophorone, cyclohexanone, ethylene glycol butyl ether, ethyl acetate, propylene glycol methyl ether, propylene glycol butyl ether, dipropylene glycol methyl ether, and dipropylene glycol butyl ether.
[0013] The particle size range of the carbon fiber powder is 800-1500 mesh; the graphene powder is one or two of single-layer graphene and few-layer graphene powder, and the particle size range of the graphite powder is 20-100 mesh; the particle size of the nano zinc oxide is about 100-500nm; the particle size of the nano titanium oxide is about 10-100nm; the particle size of the silicon carbide, niobium carbide and boron nitride is 1-10μm; the zinc powder / aluminum powder is one or two of zinc powder and aluminum powder, the mica powder is sericite powder, and the particle size range is 800-1250 mesh; the low-melting point filler is low-melting point glass powder, the melting point range is 350-550℃, and the particle size range is 800-1000 mesh; the dispersant is one or more of linear alkylamide dispersant, polyurethane dispersant, acrylic dispersant, acetylene alcohol dispersant and branched polycarboxylic acid dispersant, and the defoamer is a mineral oil defoamer , one or more of the following silicon defoamers (organic silicon, modified silicon polyether, polydimethylsiloxane and silicon dioxide mixture), the anti-flash rust additive is a cationic salt (sodium nitrite, sodium molybdate, strontium chromate, zinc phosphate, strontium phosphosilicate, aluminum tripolyphosphate, zinc aluminum phosphate + zinc molybdate) or one or more of the following organic polymer amine anti-flash rust additives, the leveling agent is silicone oil, polyester modified polydimethylsiloxane, polydimethylsiloxane, alkyl modified silicone oxide The curing agent is one or more of the alkanes, and the curing agent is one or more of polyamide, phenolic amine, polymercaptan, ethylenediamine, hexamethylenediamine, diethylenetriamine, tetraethylenepentamine, diethylaminopropylamine, 4,4'-diaminodiphenyl sulfone, m-phenylenediamine, tetraethyl orthosilicate, silane coupling agent (KH-560, KH-550, etc.), diethylenetriamine, triethylenetetramine, organic tin (dibutyltin dilaurate, etc.), organic titanium (n-butyl titanate).
[0014] An organosilicon-niobium carbide high temperature resistant heavy anti-corrosion coating and a preparation method thereof, comprising the following steps:
[0015] Preparation of component A: Stir the silicone resin and co-solvent at a speed of 500-700 rpm for 10-20 minutes to obtain a uniform silicone resin mixed solution; then add a dispersant, carbon fiber powder, graphene powder, graphite powder, and defoaming agent and stir at a speed of 500-700 rpm for 10-20 minutes, then add zinc powder / aluminum powder, nano zinc oxide, nano titanium oxide, silicon carbide, niobium carbide, boron nitride, mica powder, low melting point filler, leveling agent, etc. and stir at a speed of 1000-1200 rpm for 10-20 minutes, and finally add an anti-flash rust additive and stir at a speed of 1000-1200 rpm for 10-20 minutes to obtain slurry A;
[0016] Preparation of component B:
[0017] Stir the curing agent and the co-solvent at a speed of 500-700 rpm for 10-20 min to obtain slurry B;
[0018] Components A and B are mixed to prepare a new heavy-duty anti-corrosion coating; slurry B is added to slurry A, stirred at a speed of 1000-1200 rpm for 20-40 minutes, and then the subsequent anti-corrosion coating brushing and spraying process is carried out; and the new organosilicon-niobium carbide high-temperature resistant heavy-duty anti-corrosion coating is prepared by curing at room temperature to 80°C for 2-10 hours.
[0019] The beneficial effects of the present invention are as follows: (1) The present invention utilizes graphene powder, carbon fiber powder, and boron nitride to achieve electrical conductivity, high temperature resistance, and corrosion resistance, and because a conductive network skeleton is formed, the amount of aluminum powder used is reduced;
[0020] (2) Niobium carbide has high melting point (3500℃), high hardness, high thermal conductivity, strong thermochemical stability and other excellent properties. It is insoluble in cold or hot hydrochloric acid, sulfuric acid, and nitric acid. As an additive, it can significantly improve the wear resistance, thermal shock resistance and corrosion resistance of anti-corrosion coatings.
[0021] (3) Nano-titanium oxide, nano-zinc oxide, silicon carbide, and boron nitride can play a role in wear resistance, high temperature resistance, and corrosion resistance. The new organic silicon-niobium carbide high temperature resistant heavy anti-corrosion coating has excellent heat resistance and corrosion resistance;
[0022] (4) In the context of the dual-carbon era, the key to achieving energy conservation and emission reduction in the cement industry is to achieve low-carbon and energy-saving production in the cement clinker production process. The organosilicon-niobium carbide high-temperature resistant heavy-duty anti-corrosion coating of the present invention can be specifically applied to cement clinker production lines, successfully filling the gap in the long-term use of anti-corrosion materials in cement kiln clinker production line equipment in China.
[0023] The present invention will be described in more detail below with reference to the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a schematic diagram of the production process of the present invention. DETAILED DESCRIPTION
[0025] The directions or positional relationships indicated by the terms "upper", "lower", "inner", "outer", "front end", "rear end", "two ends", "one end", "the other end" and the like in the application text are based on the directions or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, and are not intended to indicate or imply that the devices or elements referred to must have a specific direction, be constructed and operate in a specific direction, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance.
[0026] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "provided with", "connected", etc. should be understood in a broad sense. For example, "connected" can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0027] Example 1: Preparation of a novel organosilicon-niobium carbide high temperature resistant heavy duty anti-corrosion coating
[0028] Component A:
[0029] Silicone epoxy resin (composite silicone resin of methyl silicone resin and silicone epoxy resin in a mass ratio of 3:1): 35wt.%
[0030] Co-solvent (mixed co-solvent of n-butanol, xylene and dipropylene glycol butyl ether in a mass ratio of 5:3:2): 8wt.%
[0031] Graphene powder (few-layer graphene, average particle size 100 mesh): 0.5wt.%
[0032] Carbon fiber (carbon fiber powder with an average particle size of 1000 mesh): 1wt.%
[0033] Graphite powder (graphite powder with an average particle size of 100 mesh): 3wt.%
[0034] Nano zinc oxide (the average particle size of nano zinc oxide is about 200nm): 2wt.%
[0035] Nano titanium oxide (average particle size is about 20nm): 2wt.%
[0036] Niobium carbide (average particle size is about 5 μm): 3.5 wt.%
[0037] Silicon carbide (average particle size is about 1 μm): 2 wt.%
[0038] Boron nitride (average particle size is about 10 μm): 2 wt.%
[0039] Aluminum powder: 9wt.%
[0040] Sericite powder (average particle size is about 1000 mesh): 3wt.%
[0041] Low melting point glass powder (low melting point glass powder): 13wt.%
[0042] Dispersant (composite dispersant of polyurethane dispersant and acrylic dispersant in a mass ratio of 1:1): 1.2wt.%
[0043] Defoamer (silicon defoamer): 1.3wt.%
[0044] Triple flash rust additive (composite anti-flash rust additive of zinc phosphate and aluminum tripolyphosphate with a mass ratio of 1:2): 1.5wt.%
[0045] Leveling agent (organic modified polysiloxane): 0.5wt.%
[0046] Component B:
[0047] Co-solvent (mixed co-solvent of n-butanol, xylene and dipropylene glycol butyl ether in a mass ratio of 5:3:2): 5wt.%
[0048] Curing agent (composite curing agent of polyamide 650, silane coupling agent KH-560, diethylenetriamine and n-butyl titanate in a mass ratio of 3:4:1:2): 7.5wt.%
[0049] The preparation process of the coating includes the following steps:
[0050] (1) Preparation of Component A
[0051] According to the component ratio, it is characterized in that the silicone resin and the co-solvent are stirred at a rotation speed of 500-700 rpm for 10-20 minutes to obtain a uniform silicone resin mixed solution; then a dispersant, carbon fiber powder, graphene powder, graphite powder, and a defoaming agent are added and stirred at a rotation speed of 500-700 rpm for 10-20 minutes, and then aluminum powder, nano zinc oxide, nano titanium oxide, silicon carbide, niobium carbide, boron nitride, mica powder, low melting point filler, leveling agent, etc. are added and stirred at a rotation speed of 1000-1200 rpm for 10-20 minutes, and finally an anti-flash rust additive is added and stirred at a rotation speed of 1000-1200 rpm for 10-20 minutes to obtain slurry A.
[0052] (2) Preparation of Component B
[0053] According to the component ratio, the curing agent and the co-solvent are stirred at a rotation speed of 500-700 rpm for 10-20 minutes to obtain slurry B.
[0054] (3) Preparation of new heavy-duty anticorrosive coating by mixing components A and B
[0055] Add slurry B to slurry A, stir at 1000-1200 rpm for 20-40 minutes, and then carry out subsequent anti-corrosion coating brushing, spraying and other processes; cure at room temperature to 80°C for 2-5 hours to prepare a new type of organosilicon-niobium carbide high temperature resistant heavy anti-corrosion coating.
[0056] This embodiment can be applied by spraying, rolling, brushing, etc. After testing, its specific performance is as follows
[0057] As shown in Table 1:
[0058]
[0059] Example 2
[0060] Preparation of a new type of organosilicon-niobium carbide high temperature resistant heavy duty anticorrosion coating
[0061] Component A:
[0062] Silicone epoxy resin (composite silicone resin of methyl silicone resin and silicone epoxy resin in a mass ratio of 1:1): 40wt.%
[0063] Co-solvent (mixed co-solvent of n-butanol, xylene and dipropylene glycol butyl ether in a mass ratio of 5:3:2): 7wt.%
[0064] Graphene powder (few-layer graphene, average particle size 100 mesh): 1wt.%
[0065] Carbon fiber (carbon fiber powder with an average particle size of 1000 mesh): 1.5wt.%
[0066] Graphite powder (graphite powder with an average particle size of 100 mesh): 2wt.%
[0067] Nano zinc oxide (the average particle size of nano zinc oxide is about 200nm): 2wt.%
[0068] Nano titanium oxide (average particle size is about 20nm): 2wt.%
[0069] Niobium carbide (average particle size is about 5 μm): 3 wt.%
[0070] Silicon carbide (average particle size is about 1 μm): 1.5 wt.%
[0071] Boron nitride (average particle size is about 10 μm): 1.5 wt.%
[0072] Aluminum powder: 9wt.%
[0073] Sericite powder (average particle size is about 1000 mesh): 3wt.%
[0074] Low melting point glass powder (low melting point glass powder): 10wt.%
[0075] Dispersant (composite dispersant of polyurethane dispersant and acrylic dispersant in a mass ratio of 1:1): 1.2wt.%
[0076] Defoamer (silicon defoamer): 1.3wt.%
[0077] Triple flash rust additive (composite anti-flash rust additive of zinc phosphate and aluminum tripolyphosphate with a mass ratio of 1:2): 1.5wt.%
[0078] Leveling agent (organic modified polysiloxane): 0.5wt.%
[0079] Component B:
[0080] Co-solvent (mixed co-solvent of n-butanol, xylene and dipropylene glycol butyl ether in a mass ratio of 5:3:2): 4wt.%
[0081] Curing agent (composite curing agent of polyamide 650, silane coupling agent KH-560, diethylenetriamine, and n-butyl titanate in a mass ratio of 3:4:1:2): 8wt.%
[0082] The preparation process of the coating includes the following steps:
[0083] (1) Preparation of Component A
[0084] According to the component ratio, it is characterized in that the silicone resin and the co-solvent are stirred at a rotation speed of 500-700 rpm for 10-20 minutes to obtain a uniform silicone resin mixed solution; then a dispersant, carbon fiber powder, graphene powder, graphite powder, and a defoaming agent are added and stirred at a rotation speed of 500-700 rpm for 10-20 minutes, and then aluminum powder, nano zinc oxide, nano titanium oxide, silicon carbide, niobium carbide, boron nitride, mica powder, low melting point filler, leveling agent, etc. are added and stirred at a rotation speed of 1000-1200 rpm for 10-20 minutes, and finally an anti-flash rust additive is added and stirred at a rotation speed of 1000-1200 rpm for 10-20 minutes to obtain slurry A.
[0085] (2) Preparation of Component B
[0086] According to the component ratio, the curing agent and the co-solvent are stirred at a rotation speed of 500-700 rpm for 10-20 minutes to obtain slurry B.
[0087] (3) Preparation of new heavy-duty anticorrosive coating by mixing components A and B
[0088] Add slurry B to slurry A, stir at 1000-1200 rpm for 20-40 minutes, and then carry out subsequent anti-corrosion coating brushing, spraying and other processes; cure at room temperature to 80°C for 2-5 hours to prepare a new type of organosilicon-niobium carbide high temperature resistant heavy anti-corrosion coating.
[0089] This embodiment can be applied by spraying, rolling, brushing, etc. After testing, its specific performance is as follows
[0090] As shown in Table 1:
[0091]
[0092] (1) The present invention utilizes graphene powder, carbon fiber powder, and boron nitride to achieve electrical conductivity, high temperature resistance, and corrosion resistance, and because a conductive network skeleton is formed, the amount of aluminum powder used is reduced;
[0093] (2) Niobium carbide has high melting point (3500℃), high hardness, high thermal conductivity, strong thermochemical stability and other excellent properties. It is insoluble in cold or hot hydrochloric acid, sulfuric acid, and nitric acid. As an additive, it can significantly improve the wear resistance, thermal shock resistance and corrosion resistance of anti-corrosion coatings.
[0094] (3) Nano-titanium oxide, nano-zinc oxide, silicon carbide, and boron nitride can play a role in wear resistance, high temperature resistance, and corrosion resistance. The new organic silicon-niobium carbide high temperature resistant heavy anti-corrosion coating has excellent heat resistance and corrosion resistance;
[0095] (4) In the context of the dual-carbon era, the key to achieving energy conservation and emission reduction in the cement industry is to achieve low-carbon and energy-saving production in the cement clinker production process. The organosilicon-niobium carbide high-temperature resistant heavy-duty anti-corrosion coating of the present invention can be specifically applied to cement clinker production lines, successfully filling the gap in the long-term use of anti-corrosion materials in cement kiln clinker production line equipment in China.
[0096] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A new type of organosilicon-niobium carbide high temperature resistant heavy anti-corrosion coating, characterized by: The coating is composed of two components, A and B. Component A is composed of silicone resin, co-solvent, graphene powder, carbon nanofiber, graphite powder, nano zinc oxide, nano titanium oxide, silicon carbide, niobium carbide, boron nitride, zinc powder / aluminum powder, dispersant, defoamer, anti-flash rust additive and drying agent, and component B is composed of co-solvent and curing agent. The specific coating formula is as follows in parts by weight: Component A: organic silicon resin: 10-45wt.%, cosolvent: 5-20wt.%, graphene powder: 0.1-2wt.%, carbon fiber powder: 0.1-2wt.%, graphite powder: 1-5wt.%, nano titanium oxide: 1-10wt.%, nano zinc oxide: 1-10wt.%, silicon carbide: 1-10wt.%, niobium carbide: 1-10wt.%, boron nitride: 1-10wt.%, zinc powder / aluminum powder: 5-20wt.%, mica powder: 1-10wt.%, low melting point filler: 5-30wt.%, dispersant: 0.2-3wt.%, defoamer: 0.2-3wt.%, anti-flash rust additive: 0.2-3wt.%, leveling agent: 0.2-3wt.%; Component B: cosolvent: 5-15wt.%, curing agent: 5-15wt.%; Add component B to component A and cure at room temperature to 80°C for 2-10 hours to prepare a new type of organosilicon-niobium carbide high temperature resistant heavy anti-corrosion coating.
2. The novel organosilicon-niobium carbide high temperature resistant heavy anti-corrosion coating according to claim 1, characterized in that: The silicone resin is one or more of pure silicone resin (polysilazane or polysiloxane), methyl silicone resin, methylphenyl silicone resin, silicone polyester resin, silicone alkyd resin, silicone acrylic resin and silicone epoxy resin.
3. The novel organosilicon-niobium carbide high temperature resistant heavy anti-corrosion coating according to claim 1, characterized in that: The co-solvent is one or more of methanol, ethanol, toluene, xylene, trimethylbenzene, n-butanol, 1,4-butanediol, acetone, isophorone, cyclohexanone, ethylene glycol butyl ether, ethyl acetate, propylene glycol methyl ether, propylene glycol butyl ether, dipropylene glycol methyl ether, and dipropylene glycol butyl ether.
4. The novel organosilicon-niobium carbide high temperature resistant heavy anti-corrosion coating according to claim 1, characterized in that: The particle size range of the carbon fiber powder is 800-1500 mesh; the graphene powder is one or two of single-layer graphene and few-layer graphene powder, and the particle size range of the graphite powder is 20-100 mesh; the particle size of the nano zinc oxide is about 100-500nm; the particle size of the nano titanium oxide is about 10-100nm; the particle size of the silicon carbide, niobium carbide, and boron nitride is 1-10μm; the zinc powder / aluminum powder is one or two of zinc powder and aluminum powder, the mica powder is sericite powder, and the particle size range is 800-1250 mesh; the low-melting point filler is low-melting point glass powder, the melting point range is 350-550℃, and the particle size range is 800-1000 mesh; the dispersant is a linear alkylamide dispersant, a polyurethane dispersant, a polyurethane dispersant, a polyurethane prepolymer, a polyurethane prepolymer, a polyurethane prepolymer, a polyurethane prepolymer, a polyurethane prepolymer, a polyurethane prepolymer, a polyurethane prepolymer, a polyurethane prepolymer, a polyurethane prepolymer, a polyurethane prepolymer, a polyurethane prepolymer, a polyurethane prepolymer, a polyurethane prepolymer, a polyurethane prepolymer, a polyurethane prepolymer, a polyurethane prepolymer, a polyurethane prepolymer, a polyurethane prepolymer, a polyurethane prepolymer, a polyurethane prepolymer, a polyurethane prepolymer, The invention discloses a kind of polyol dispersant, ...
5. An organosilicon-niobium carbide high temperature resistant heavy anti-corrosion coating and a preparation method thereof, characterized in that: The following steps are involved: Preparation of component A: Stir the silicone resin and co-solvent at a speed of 500-700 rpm for 10-20 minutes to obtain a uniform silicone resin mixed solution; then add a dispersant, carbon fiber powder, graphene powder, graphite powder, and defoaming agent and stir at a speed of 500-700 rpm for 10-20 minutes, then add zinc powder / aluminum powder, nano zinc oxide, nano titanium oxide, silicon carbide, niobium carbide, boron nitride, mica powder, low melting point filler, leveling agent, etc. and stir at a speed of 1000-1200 rpm for 10-20 minutes, and finally add an anti-flash rust additive and stir at a speed of 1000-1200 rpm for 10-20 minutes to obtain slurry A; Preparation of component B: Stir the curing agent and co-solvent at a speed of 500-700 rpm for 10-20 min to obtain slurry B; Components A and B are mixed to prepare a new heavy-duty anti-corrosion coating; slurry B is added to slurry A, stirred at a speed of 1000-1200 rpm for 20-40 minutes, and then the subsequent anti-corrosion coating brushing and spraying process is carried out; and the new organosilicon-niobium carbide high-temperature resistant heavy-duty anti-corrosion coating is prepared by curing at room temperature to 80°C for 2-10 hours.
Citation Information
Patent Citations
High-heat-conductivity, high-temperature-resisting and heavy-duty anti-corrosive coating and preparation method thereof
CN108395808A
High-temperature-resistant graphene rapid heat dissipation anticorrosive coating as well as preparation method and application thereof
CN111171708A
Preparation method of organosilicon high-temperature-resistant anticorrosive paint
CN112625594A
Protective coating for repairing metal surface damage, preparation method and composite material
CN113914277A
High-temperature-resistant normal-temperature curing type anticorrosive paint, preparation method and application
CN114381203A
Cited By
Wear-resistant anti-corrosion tungsten steel material and processing technology thereof
CN122037708A