Microstructure self-healing super-hydrophobic coating, preparation method and application

By using diatomaceous earth and dopamine encapsulated octamine, combined with bisamino-terminated polydimethoxysilane, a microstructure self-healing superhydrophobic coating is formed, which solves the durability and environmental friendliness of the superhydrophobic coating. Problem, efficient coating recovery and wide application.

CN118931383AActive Publication Date: 2024-11-12SOUTHWEST JIAOTONG UNIV

Patent Information

Application Number
CN202411219519.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-12
Estimated Expiration
2044-09-02

AI Technical Summary

Technical Problem

The durability of existing superhydrophobic coatings is insufficient, especially under chemical and physical damage, microstructure self-repair studies are rarely studied, and commonly used materials such as graphene and fluoroelastic resins are costly and unfriendly and environmentally unfriendly.

Method used

Using diatomaceous earth as the matrix, octadecamine is encapsulated by dopamine and combined with bisamino-terminated polydimethoxysilane to form a microstructure self-healing superhydrophobic coating. It is mass-produced by spray coating to achieve hydrophobic coating. Modification and self-healing.

Benefits of technology

It reduces the cost of coating preparation and improves the recovery rate of microstructure. The recovery rate of coating after damage is as high as 98.6%, and uses environmentally friendly materials, suitable for a wide range of industrial and daily applications, and enhances the adhesion strength of the matrix material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931383A_ABST
    Figure CN118931383A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of super-hydrophobic coatings, and particularly relates to a microstructure self-healing super-hydrophobic coating, a preparation method and application. The preparation method comprises the following steps: calcining diatomite, adding the calcined diatomite into a NaOH solution to obtain diatomite A, mixing the diatomite A with an octadecylamine liquid, carrying out vacuum impregnation to obtain diatomite DO impregnated with octadecylamine, adding the DO into a solvent, adjusting the pH value, and adding dopamine to obtain DOA; the preparation method comprises the following steps: adding DOA into a solvent, and adding bis-amino-terminated polydimethoxysilane, so as to obtain N-DOA; the preparation method comprises the following steps: adding N-DOA, NH2-PDMS (Polydimethylsiloxane)-NH2 and acrylic resin into a butyl acetate solution, then adding benzaldehyde to obtain a mixed solution, and then preparing the microstructure self-healing super-hydrophobic coating on a base material through a spray gun. The coating is high in microstructure recovery rate and low in preparation cost, and fluoride-free modification is achieved through the preparation method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of super hydrophobic coatings, and in particular relates to a microstructured self-healing super hydrophobic coating, a preparation method and an application thereof. Background Art

[0002] The hydrophobicity of super-hydrophobic coatings depends on low surface energy and surface micro-nanostructures, but in practical applications, due to chemical and physical effects, the low surface energy and micro-nanostructures are damaged, resulting in the Cassie-Wenzel transition of droplets. Therefore, the durability of super-hydrophobic coatings limits their practical applications.

[0003] In order to solve the durability problem of superhydrophobic coatings, current research mainly focuses on enhancing the mechanical strength of the coating itself and self-repair of damage. Among them, self-healing coatings are widely studied because they can repair damage by themselves, including self-healing coatings that store low surface energy substances in porous capsules, phase change movement of low melting point substances, and use of intermolecular kinetic bonds to promote thermal motion of chain segments. For chemical damage, self-repair can be achieved by releasing low surface energy substances or thermal motion of molecular segments to replace the generated polar groups, but there is little research on self-repair of microstructures.

[0004] Liu et al. prepared a microstructure self-repairing super-hydrophobic coating by the thermal expansion of graphene and the elastic deformation characteristics of fluororubber resin (FKM). Zhang et al. used carnauba wax (CW) as the temperature-responsive phase change material of the super-hydrophobic coating, combined with modified fluororubber (MFR) and carbon nanofiber (CNF) with a large aspect ratio, and obtained a super-hydrophobic FSR / CNF / CW / MFR composite coating with excellent structural repair performance, effectively improving the hydrophobic stability and service life of the super-hydrophobic coating. Therefore, the present invention encapsulates the 18-phase change material in porous diatomite by the self-oxidative polymerization of dopamine, and after modification by diamino-terminated PDMS, it is dispersed in an acrylic resin and PDMS mixed solution, and a super-hydrophobic coating with microstructure self-repair is prepared by a simple spraying method.

[0005] At present, microstructure self-healing superhydrophobic coatings have been prepared by using the thermal expansion of graphene (EAG) and the elastic deformation properties of fluororubber resin (FKM). The main steps are to first synthesize fluorine-modified graphene nanoparticles, evenly disperse 0.25g EAG and 2m LTEOS in 20mL ethanol, mechanically stir for 10min, and dropwise add a mixture of 2m NH3·H2O and 20mL ethanol to the above solution, stirring at 300r / min for 12h. Then, 100μL 1H, 1H, 2H, 2H-perfluorodecyltrichlorosilane (PFTS) was added to the EAG@SiO2 gel, and after hydrolysis for 12h, the EAG@SiO2-PFTS particles were obtained by drying at 80℃. During the calcination process of the coating, rich micro-nanostructures can be constructed to achieve superhydrophobic properties.

[0006] Then the super-hydrophobic coating was prepared: first, 1.0g polyphenylene sulfide (PPS) resin powder was dispersed in 10mL ethanol, and then the suspension was sprayed on the polished aluminum substrate with an air spray gun at a pressure of 6bar, and the spraying distance was kept at 15-20cm. After calcination at 300°C, the bottom pure PPS coating was obtained to enhance the adhesion of the subsequent super-hydrophobic coating. Subsequently, 0.04g EAG@SiO-PFTS, 0.08g FKM, 1.0gPPS, and 0.1g FEP were dispersed in 10mL ethanol and magnetically stirred for 1h to prepare a super-hydrophobic polymer suspension. Finally, the prepared suspension was sprayed on the surface of the pre-coated PPS coating. During the heat treatment at 300°C, a super-hydrophobic PPS / FKM / EG@SiO2 coating was obtained, and the coating rapidly expanded from EAG@SiO2 to EG@SiO2. However, the use of graphene to make super-hydrophobic coatings is costly, and the introduction of fluorosilane for hydrophobic modification causes fluorine poisoning, which is not environmentally friendly.

[0007] Preparation of CW and MFR composite particles: A mixed solution of 4g carnauba wax (CW) and 40mL ethyl acetate was placed in a reagent bottle and vigorously stirred in an 85°C water bath for 5 minutes. Subsequently, 20mL ethanol was added dropwise to the CW / ethyl acetate mixed solution at room temperature and stirred. After cooling, vacuum filtration and drying, CW particles were obtained. 0.16g fluororubber (FR) particles were added to a mixture of 40μL POTS and 1mL ethyl acetate. The FR particles expanded slightly while being impregnated and modified. Finally, fluorosilane-modified fluororubber particles were obtained by drying at 80°C, named MFR.

[0008] Preparation of super-hydrophobic coating: CNF (0.12g) and MFR (0.12g) particles were dispersed in ethyl acetate (15mL) under strong ultrasonic vibration for 10min. Subsequently, FSR resin (1g), N3390 curing agent (1g) and CW powder (0.05g) were added to the solution and dispersed under strong ultrasonic vibration using an ultrasonic generator for 5min. Finally, the solution was sprayed on the treated aluminum plate at a pressure of 5-6bar under a heating platform at 40°C. After curing at 180°C for 1h in a blast drying oven, a super-hydrophobic FSR / CNF / CW / MFR coating was successfully obtained, but the cost of using carbon nanofibers to construct a network structure is high, which is not easy to be widely used in super-hydrophobic coatings. The use of fluorosilane for hydrophobic modification is environmentally unfriendly. The phase change material carnauba wax used leaks when the temperature exceeds its melting point, which reduces the cycle life of the coating; therefore, a microstructure self-healing super-hydrophobic coating, preparation method and application are urgently needed. Summary of the invention

[0009] In view of the problems and shortcomings in the prior art, the present invention provides a method for preparing a microstructured self-healing super-hydrophobic coating, comprising the following steps:

[0010] S1: calcining diatomaceous earth, adding it to a NaOH solution, stirring, filtering and drying to obtain diatomaceous earth A;

[0011] S2: mixing diatomite A and octadecylamine liquid in a mass ratio of 2:1, and performing vacuum impregnation to obtain diatomite DO impregnated with octadecylamine;

[0012] S3: adding the diatomaceous earth DO obtained in step 2 to the solvent, adjusting the pH, stirring, adding dopamine, continuing to stir, and drying to obtain dopamine-encapsulated DOA;

[0013] S4: adding the DOA obtained in step 3 to a solvent, adding diamino-terminated polydimethoxysilane, stirring and washing, and vacuum drying to obtain polydimethoxysilane-modified N-DOA;

[0014] S5: Add the N-DOA obtained in step 4, polydimethoxysilane and acrylic resin to the butyl acetate solution and stir, add benzaldehyde and continue stirring to obtain a mixed liquid, use a spray gun to spray the mixed liquid on the base material under pressure, and cure it to obtain a microstructure self-healing super hydrophobic coating.

[0015] Furthermore, the calcination time described in S1 is 2 hours, and the calcination temperature is 600°C.

[0016] Furthermore, the stirring time described in S1 is 2 hours, the stirring temperature is 75° C., the drying temperature is 80° C., and the drying time is 2 hours.

[0017] Furthermore, the immersion temperature in S2 is 70° C. and the immersion time is 1 h.

[0018] Furthermore, in S3, the pH is adjusted to 8.5, the stirring time is 1 to 2 hours, the drying time is 2 hours, and the drying temperature is 60°C.

[0019] Furthermore, the stirring time in S4 is 12 h.

[0020] Furthermore, in S5, the stirring time is 10 min, the curing temperature is 80° C., the curing time is 1 h, and the pressure is 0.5 MPa.

[0021] A microstructured self-healing super-hydrophobic coating, wherein the coating is a lotus leaf-like coating structure with a micro-nano-scale papillary structure.

[0022] The invention discloses an application of a microstructured self-healing super-hydrophobic coating, wherein the coating is applied in the preparation of a self-cleaning, anti-icing and anti-fouling coating.

[0023] Technical Effects

[0024] (1) The present invention provides a microstructure self-healing super hydrophobic coating, which uses diatomaceous earth and octadecylamine at a favorable price to reduce the coating preparation cost, and the microstructure recovery rate of the coating is high. After being rubbed with 600-grit sandpaper for 2000 cm, the damaged structure is restored under the action of octadecylamine phase change and molecular chain segment movement, and the super hydrophobicity recovery rate is as high as 98.6%; and the coating is greener.

[0025] (2) The present invention provides a method for preparing a microstructured self-healing super hydrophobic coating, which can be prepared on a large scale, wherein a simple spraying method realizes the large-scale preparation of the coating. The preparation method uses NH2-PDMS-NH2 to perform hydrophobic modification of the coating, which not only enhances the dispersibility of DOA in the matrix material, but also realizes fluorine-free modification.

[0026] (3) The application of the microstructured self-healing super-hydrophobic coating provided by the present invention has a wide range of applications. Using AR / NH2-PDMS-NH2 as the matrix material enhances the adhesion strength between the coating and a variety of substrate materials, thus broadening its application. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the technical solutions of the exemplary embodiments of the present invention, the following is a brief introduction to the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present invention and should not be regarded as limiting the scope. For those of ordinary skill in the art, other relevant drawings can be obtained based on these drawings without creative work. In the drawings:

[0028] Figure 1 The graphs are of the contact angle changes of the coating of Example 1 of the present invention before and after being abraded by 600-mesh sandpaper and after light healing.

[0029] Figure 2 The graphs show the changes in the surface morphology of the coating of Example 1 of the present invention before and after being abraded by 600-mesh sandpaper and after light healing.

[0030] Figure 3 Schematic diagram of the preparation process of the phase change capsule (a) and the photothermal self-healing superhydrophobic coating (b) of Example 1 of the present invention. DETAILED DESCRIPTION

[0031] The following will be combined with Example 1 of the present invention and the attached Figures 1 to 3, the technical solution of the present invention is clearly and completely described. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] The present invention provides a method for preparing a microstructured self-healing super-hydrophobic coating, comprising the steps of first calcining Changbai Mountain diatomite in a muffle furnace, then adding it to a NaOH solution, stirring and filtering, and then putting it into a vacuum drying oven to dry, so as to obtain diatomite A; then mixing diatomite A with octadecylamine (PCM) liquid in a mass ratio of 2:1, and then putting it into a vacuum drying oven for impregnation, so as to obtain diatomite DO impregnated with octadecylamine; then adding DO to a deionized water solution, adjusting the solution pH, stirring at room temperature, adding dopamine and continuing to stir, and drying in a vacuum drying oven to obtain dopamine-encapsulated DO (DOA), S3 selects dopamine to encapsulate octadecylamine, which not only gives the coating photothermal properties, but also promotes octadecylamine to undergo phase change and repair the damaged microstructure;

[0033] DOA is added to an ethanol solution, and then an equal amount of bisamino-terminated polydimethoxysilane (NH2-PDMS-NH2) is added. After stirring at room temperature, the mixture is washed three times with an ethanol solution and vacuum dried to obtain NH2-PDMS-NH2-modified DOA (N-DOA). The formed polydopamine undergoes a Schiff base reaction with the bisamino-terminated polydimethoxysilane in step S4, and the bisamino-terminated polydimethoxysilane is grafted onto the surface of DOA, which not only plays a hydrophobic role, but also the dynamic imine bond formed under the action of BTC promotes the movement of DOA along the molecular chain segment, further promoting microstructure repair.

[0034] After adding N-DOA, NH2-PDMS-NH2 and AR to butyl acetate solution and stirring, benzaldehyde (BTC) was added and continued to stir. Then, the obtained mixed solution was sprayed on the substrate material using a spray gun at a pressure of 0.5 MPa, and a microstructured self-healing superhydrophobic coating was obtained after curing.

[0035] Example 1

[0036] S1: 5 g of Changbai Mountain diatomite was calcined in a muffle furnace at 600°C for 2 h, then added into a 1 mol / L NaOH solution, stirred at 75°C for 2 h, filtered, and dried in a vacuum drying oven at 80°C for 2 h to obtain diatomite A;

[0037] S2: The diatomite A obtained in S1 was mixed with octadecylamine (PCM) liquid in a mass ratio of 2:1, and immersed in a vacuum drying oven at 70°C and 0.8 MPa for 1 h to obtain diatomite DO impregnated with octadecylamine;

[0038] S3: Add the DO obtained in S2 to 20 ml of deionized water solution, adjust the solution pH to 8.5, stir at room temperature for 1 hour, then add 50 wt% dopamine and continue stirring for 2 hours, and dry in a vacuum oven at 60°C for 2 hours to obtain dopamine-encapsulated DO (DOA);

[0039] S4: Add the DOA obtained in S3 to an ethanol solution, then add an equal amount of diamino-terminated polydimethoxysilane (NH2-PDMS-NH2), stir at room temperature for 12 hours, wash three times with an ethanol solution, and vacuum dry to obtain NH2-PDMS-NH2-modified DOA (N-DOA);

[0040] S5: Add N-DOA, NH2-PDMS-NH2 and AR obtained in S4 to butyl acetate solution and stir for 10 minutes, then add 2-benzaldehyde (BTC) and continue stirring for 10 minutes. Use a 0.5 mm spray gun at a pressure of 0.5 MPa to spray the resulting mixed solution on the substrate material, and cure it at 80°C for 1 hour to obtain a microstructured self-healing super hydrophobic coating.

[0041] from Figure 1 It can be seen that under a load of 200g, after rubbing for 2000cm, the contact angle decreased from 159.7° to 149.2°, indicating that the microstructure was damaged during the friction process, resulting in an increase in the solid-liquid contact area and a decrease in the contact angle. After 20 minutes of illumination, the contact angle recovered to 158.9°. The photothermal effect of the coating promoted the movement of the NH2-PDMS-NH2 chain segment. At the same time, the damaged diatomaceous earth released octadecylamine, which underwent a phase change, further promoting the repair of the microstructure, so the contact angle increased.

[0042] from Figure 2 It can be seen that after the coating is worn, the surface microstructure is partially worn away. After exposure to light, a new microstructure appears on the smoothed surface due to the movement of the NH2-PDMS-NH2 chain segments and the phase change of octadecylamine, thus repairing the damaged surface microstructure.

[0043] from Figure 3 It can be seen that in order to prevent the leakage of phase change materials, octadecylamine is encapsulated in the high-strength diatomite pores through dopamine, as shown in Figure (a). The diatomite pore size is increased by calcination and alkali treatment, and then octadecylamine is encapsulated in the diatomite pores by vacuum impregnation. After being coated with dopamine, it not only gives the phase change capsule photothermal properties, but also facilitates the hydrophobic modification of NH2-PDMS-NH2. The preparation process of the coating is shown in Figure (b). After AR, PDMS, BTC and N-DOA are added to butyl acetate solution and stirred, they are evenly sprayed on the substrate surface with a spray gun, and a self-healing super hydrophobic coating is obtained after drying.

[0044] The present invention provides a microstructured self-healing super-hydrophobic coating based on diatomite and octadecylamine, which greatly reduces the preparation cost. The coating has excellent self-healing properties. After being rubbed for 2000 cm with 600-mesh sandpaper, it can still restore its microstructure under the phase change and molecular segment movement of octadecylamine, with a recovery rate of up to 98.6%, showing excellent durability and damage resistance. In addition, the present invention pays attention to environmental protection, and the coating uses greener and more sustainable materials, which further reduces the impact on the environment, making it more advantageous in practical applications.

[0045] By the preparation method of a kind of microstructure self-healing super hydrophobic coating provided by the present invention, the preparation method is not only simple and economical, but also particularly suitable for large-scale production. By simple spraying process, self-healing super hydrophobic coating can be efficiently and uniformly generated on large-area substrates. The method adopts NH2-PDMS-NH2 as the hydrophobic modifier of coating, not only enhances the dispersibility of octadecylamine (DOA) in matrix material, but also realizes fluorine-free modification, so that the whole preparation process is more green and environmentally friendly, meets the demand of modern industry for environmentally friendly materials.

[0046] By the application of a preparation method of a microstructure self-healing super-hydrophobic coating provided by the present invention, the microstructure self-healing super-hydrophobic coating of the present invention has a wide range of applications. Using AP / NH2-PDMS-NH2 as a matrix material, the adhesion strength between the coating and a variety of substrate materials is greatly improved, making it suitable for a variety of industrial fields, including aerospace, automobile manufacturing, electronic equipment, etc. At the same time, the coating material of the present invention has excellent wear resistance and antifouling properties, and shows extremely high reliability and long-term effectiveness in practical applications. This wide applicability makes it have broad prospects in industry and daily life.

Claims

1. A method for preparing a microstructured self-healing super-hydrophobic coating, characterized in that: The following steps are involved: S1: calcining diatomaceous earth, adding it to a NaOH solution, stirring, filtering and drying to obtain diatomaceous earth A; S2: mixing diatomite A and octadecylamine liquid in a mass ratio of 2:1, and performing vacuum impregnation to obtain diatomite DO impregnated with octadecylamine; S3: adding the diatomaceous earth DO obtained in step 2 to the solvent, adjusting the pH, stirring, adding dopamine, continuing to stir, and drying to obtain dopamine-encapsulated DOA; S4: adding the DOA in step 3 to a solvent, adding diamino-terminated polydimethoxysilane, stirring and washing, and vacuum drying to obtain polydimethoxysilane-modified N-DOA; S5: Add the N-DOA obtained in step 4, polydimethoxysilane and acrylic resin to the butyl acetate solution and stir, add benzaldehyde and continue stirring to obtain a mixed liquid, use a spray gun to spray the mixed liquid on the base material under pressure, and cure it to obtain a microstructure self-healing super hydrophobic coating.

2. A method for preparing a microstructured self-healing super-hydrophobic coating according to claim 1, characterized in that, The calcination time described in S1 is 1 to 3 hours, and the calcination temperature is 600°C.

3. A method for preparing a microstructured self-healing super-hydrophobic coating according to claim 1, characterized in that, The stirring time described in S1 is 2 hours, the stirring temperature is 75° C., the drying temperature is 80° C., and the drying time is 2 hours.

4. A method for preparing a microstructured self-healing super-hydrophobic coating according to claim 1, characterized in that, In S2, the immersion temperature is 70° C. and the immersion time is 1 hour.

5. A method for preparing a microstructured self-healing super-hydrophobic coating according to claim 1, characterized in that: In S3, the pH is adjusted to 8.5, the stirring time is 1 to 2 hours, the drying time is 2 hours, and the drying temperature is 60°C.

6. The method for preparing a microstructured self-healing super-hydrophobic coating according to claim 1, characterized in that: The stirring time in S4 is 12 h.

7. The method for preparing a microstructured self-healing super-hydrophobic coating according to claim 1, characterized in that: In S5, the stirring time is 10 min, the curing temperature is 80° C., the curing time is 1 h, and the pressure is 0.5 MPa.

8. A microstructured self-healing super-hydrophobic coating obtained by the preparation method according to any one of claims 1 to 7, characterized in that: The coating is a lotus leaf-like coating structure with a micro-nano-scale papillary structure.

9. The use of a microstructure self-healing super-hydrophobic coating according to claim 8, characterized in that: The coating is used in preparing self-cleaning, anti-icing and anti-fouling coatings.

Citation Information

Patent Citations

  • Self-repairing super-hydrophobic composite material, preparation method and application thereof

    CN105949861A

  • Preparation method of organic silicon self-repair antifouling material

    CN108546337A

  • Wearing-resistant super-hydrophobic fabric and preparation method thereof

    CN109610179A

  • Method for preparing super-hydrophobic paper through laser printing

    CN112522991A

  • Self-repairing super-hydrophobic coating and preparation method thereof

    CN112778905A

Cited By

  • Photo-thermal anti-icing and deicing super-hydrophobic coating with three-dimensional network structure and preparation method thereof

    CN119391242A

  • Double-layer composite high-breathability low-sensitivity adhesive tape and preparation method thereof

    CN119979043A