Substrate-free adhesive film and preparation process thereof

Through the design of the baseless adhesive film, combined with the silicone adhesive layer, the basecoat layer and the polyacrylate adhesive layer, the problems of arching and separation of the adhesive film during bending are solved, the production process is simplified, and the environmental protection is improved. .

CN118931396APending Publication Date: 2024-11-12江苏晶华新材料科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411228420.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing adhesive film has strong bending rebound force when it is bent on curved surfaces, concave and convex surfaces, and when it is bent, it is easy to arch and curl, resulting in separation of the glue and silicon foam, and the production process is complicated and not environmentally friendly.

Method used

The baseless film design is adopted, including a layered silicone adhesive layer, a primer layer and a polyacrylate adhesive layer, which is prepared through specific raw material components and process steps to avoid the problems of arches and separation caused by the substrate, and Simplified production process.

Benefits of technology

The separation of the adhesive film and silicon foam is effectively avoided, production costs are reduced, and the pulling strength of the substrate-free adhesive film is greater than 2MPa, solving the problem of difficult degradation and treatment of substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931396A_ABST
    Figure CN118931396A_ABST
Patent Text Reader

Abstract

The invention discloses a substrate-free adhesive film and a preparation process thereof, and the substrate-free adhesive film comprises a silica gel adhesive layer, a priming coat and a polyacrylate adhesive layer which are arranged in a laminated manner, the bottom coating is prepared from the following raw material components in parts by mass: 10 to 22 parts of a film-forming agent, 11 to 26 parts of a coupling agent, 5 to 10 parts of a catalyst and 30 to 60 parts of a diluent. According to the substrate-free adhesive film and the preparation process thereof disclosed by the invention, the bad problems caused by the substrate can be avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of adhesive films, and in particular relates to an adhesive film without a substrate and a preparation process thereof. Background Art

[0002] Silicone foam is widely used in new energy vehicle battery packs, 5G communications, restraint trays, electronic appliances, high-speed rail, aviation and other industries because of its good shock absorption, heat insulation, sealing, filling, flame retardant insulation and edge protection properties. It usually needs to be used with adhesive backing. Because of its low surface energy, it usually needs to be primed on the surface before being attached with acrylic PET double-sided tape.

[0003] However, in actual application, the following problems also exist: (1) The adhesive film has a substrate. When it is attached to a curved surface, an uneven surface, or when it is bent, the substrate has a strong bending rebound force, which can easily cause arching and warping, resulting in separation of the adhesive and the silicone foam; (2) The production process of double-sided adhesive films with substrates is complicated, requiring multiple laminations of the substrates, and the bonding strength between silicone and PET substrates is poor, requiring primer treatment, and the cost of the entire process is also higher; (3) The substrate in the adhesive film is difficult to degrade and treat, which is not environmentally friendly.

[0004] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention

[0005] The object of the present invention is to provide a substrate-free adhesive film and a preparation process thereof, which can provide a substrate-free adhesive film, thereby avoiding the adverse problems caused by the substrate.

[0006] In order to achieve the above-mentioned purpose, a technical solution provided by a specific embodiment of the present invention is as follows: a substrate-free adhesive film, comprising a laminated silicone adhesive layer, a primer layer, and a polyacrylate adhesive layer; the primer layer comprises the following raw material components by mass: 10 to 22 parts of a film-forming agent, 11 to 26 parts of a coupling agent, 5 to 10 parts of a catalyst, and 30 to 60 parts of a diluent.

[0007] In one or more embodiments of the present invention, the film-forming agent includes acrylic modified silicone resin and polymethyl hydrogen siloxane, and the mass ratio of the acrylic modified silicone resin to the polymethyl hydrogen siloxane is (5-10):(5-12).

[0008] In one or more embodiments of the present invention, the coupling agent includes γ-(2,3-epoxypropoxy)propyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane and vinyltriethoxysilane, and the mass ratio of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane and vinyltriethoxysilane is (3-8): (3-10): (5-8).

[0009] In one or more embodiments of the present invention, the catalyst includes tetrabutyl titanate and γ-isocyanatepropyltriethoxysilane, and the mass ratio of tetrabutyl titanate to γ-isocyanatepropyltriethoxysilane is (3-5): (2-5).

[0010] In one or more embodiments of the present invention, the diluent includes at least one of toluene, ethyl acetate, butanone, and solvent oil.

[0011] In one or more embodiments of the present invention, the primer layer comprises the following raw material components by weight:

[0012] 5-10 parts of acrylic modified silicone resin, 5-12 parts of polymethyl hydrogen siloxane, 3-8 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, 3-10 parts of γ-methacryloxypropyltrimethoxysilane, 5-8 parts of vinyltriethoxysilane, 3-5 parts of tetrabutyl titanate, 2-5 parts of γ-isocyanatepropyltriethoxysilane, and 30-60 parts of diluent.

[0013] In one or more embodiments of the present invention, the substrate-free adhesive film further comprises a fluoroplastic release film, and the fluoroplastic release film is attached to a side of the silicone adhesive layer that is away from the primer layer.

[0014] In one or more embodiments of the present invention, the substrate-free adhesive film further comprises a high-release-force release film, and the high-release-force release film is attached to a side of the polyacrylate adhesive layer that is away from the primer layer.

[0015] In one or more embodiments of the present invention, the thickness of the substrate-free adhesive film is 30 to 300 μm, and the pull-out strength of the substrate-free adhesive film is greater than 2 MPa;

[0016] The thickness of the silicone adhesive layer is 5 to 50 μm;

[0017] The thickness of the polyacrylate adhesive layer is 20 to 200 μm.

[0018] A specific embodiment of the present invention further provides a process for preparing the substrate-free adhesive film as described above, comprising the following steps:

[0019] The film-forming agent, coupling agent and diluent in the raw materials of the primer layer are mixed in proportion, heated and mixed evenly, and then a catalyst is added to obtain a primer after reaction;

[0020] Applying polyacrylate adhesive on the release film, and forming a polyacrylate adhesive layer on the release film after heating and drying;

[0021] A layer of primer is sprayed on the polyacrylate adhesive layer, and after drying, a primer layer is obtained on the polyacrylate adhesive layer;

[0022] Applying silicone adhesive on the release film, and heating and drying to form a silicone adhesive layer on the release film;

[0023] The silicone adhesive layer is laminated to the primer layer to obtain a substrate-free adhesive film.

[0024] Compared with the prior art, the substrate-free adhesive film of the present invention has the following beneficial effects:

[0025] (1) It avoids the problem of bulging and warping caused by the adhesive film having a substrate in the double-sided tape, which causes the adhesive and the silicone foam to separate;

[0026] (2) The preparation process is simplified, the preparation steps are reduced, and the preparation cost is reduced;

[0027] (3) The problem that the substrate in the film is difficult to degrade and treat, which is not environmentally friendly, is solved. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0029] Figure 1 The flowchart of the preparation process of the substrate-free adhesive film in one example of the present invention is shown. DETAILED DESCRIPTION

[0030] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0031] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0032] The substrate-free adhesive film in one embodiment of the present invention comprises a silicone adhesive layer, a primer layer, and a polyacrylate adhesive layer which are stacked; the primer layer comprises the following raw material components by weight: 10 to 22 parts of a film-forming agent, 11 to 26 parts of a coupling agent, 5 to 10 parts of a catalyst, and 30 to 60 parts of a diluent.

[0033] Preferably, the film-forming agent comprises acrylic modified silicone resin and polymethyl hydrogen siloxane, and the mass ratio of the acrylic modified silicone resin to the polymethyl hydrogen siloxane is (5-10):(5-12).

[0034] Among them, the film-forming agent can form a film on the surface of the material and provide basic support. Acrylic modified silicone resin can form a silane end with one end combined with silica gel with polymethyl hydrogen siloxane, and the other end contains a methyl group of acrylic acid, which is easier to combine with similar acrylic resins; polymethyl hydrogen siloxane can be combined with acrylic modified silicone resin, and can also react with a silane coupling agent to form a silane end that can be combined with silica gel at one end, and the other end contains different highly reactive functional groups, which can be combined with a variety of acrylic resins containing incompatible groups, and has higher adaptability. Specifically. Acrylic modified silicone resin can be SH-656874 sold by Sihai Company.

[0035] The polyacrylate adhesive layer can be made of polyacrylate adhesive. Specifically, the polyacrylate adhesive can be W-983 high viscosity glue produced by Jinghua.

[0036] The silicone adhesive layer can be made of silicone adhesive, which can be SO-024 silicone glue produced by Jinghua.

[0037] Preferably, the coupling agent includes γ-(2,3-epoxypropoxy)propyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane and vinyltriethoxysilane, and the mass ratio of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane and vinyltriethoxysilane is (3-8):(3-10):(5-8).

[0038] Silane coupling agent contains two functional groups with different chemical properties. The silane end can have good bonding with silica gel, and the other end has high reactivity and can react with a variety of acrylic resins. Different coupling agents have different reactive groups and are more compatible with acrylic resins.

[0039] The catalyst in the present invention can also be called a cross-linking agent, which plays a role in catalyzing / cross-linking reactions and promoting the reaction between the film-forming agent and the coupling agent.

[0040] Preferably, the catalyst comprises tetrabutyl titanate and γ-isocyanatepropyltriethoxysilane, and the mass ratio of tetrabutyl titanate to γ-isocyanatepropyltriethoxysilane is (3-5):(2-5).

[0041] The diluent in the present invention can be compatible (soluble) with other raw material components, reduce the viscosity of the finished product, and is suitable for coating. Specifically, the diluent includes at least one of toluene, ethyl acetate, butanone, and solvent oil.

[0042] Preferably, the primer layer comprises the following raw material components by weight:

[0043] 5-10 parts of acrylic modified silicone resin, 5-12 parts of polymethyl hydrogen siloxane, 3-8 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, 3-10 parts of γ-methacryloxypropyltrimethoxysilane, 5-8 parts of vinyltriethoxysilane, 3-5 parts of tetrabutyl titanate, 2-5 parts of γ-isocyanatepropyltriethoxysilane, and 30-60 parts of diluent.

[0044] In a specific embodiment, the substrate-free adhesive film further comprises a fluoroplastic release film, which is attached to the side of the silicone adhesive layer that is away from the primer layer. Specifically, the fluoroplastic release film can be F5010 produced by Yuancai Company.

[0045] In a specific embodiment, the substrate-free adhesive film further comprises a high release force release film, which is attached to the side of the polyacrylate adhesive layer away from the primer layer. Specifically, the high release force release film can be a JTPT50D-R4 single-sided release film produced by Jinghua Company.

[0046] In a specific embodiment, the thickness of the substrate-free adhesive film is 30-300 μm, and the pull-out strength of the substrate-free adhesive film is greater than 2 MPa; the thickness of the silicone adhesive layer is 5-50 μm; and the thickness of the polyacrylate adhesive layer is 20-200 μm.

[0047] like Figure 1 As shown, a specific embodiment of the present invention further provides a process for preparing the substrate-free adhesive film as described above, comprising the following steps:

[0048] S1. Mix the film-forming agent, coupling agent and diluent in the raw materials of the primer layer in proportion, heat and mix them evenly, then add a catalyst, and obtain the primer after reaction.

[0049] Step S1 is specifically as follows: adding the film-forming agent, coupling agent and diluent into a reaction kettle in proportion, heating to 60-90° C. and stirring for 2-4 hours, adding the catalyst / cross-linking agent after complete dissolution, stirring for another 2 hours under heat preservation conditions, mixing evenly, and sealing and storing for later use.

[0050] S2, coating the polyacrylate adhesive on the release film, and heating and drying to form a polyacrylate adhesive layer on the release film.

[0051] Specifically, the heating and drying temperature is 70 to 110° C., and the drying time is 3 to 5 minutes.

[0052] S3. Spray a layer of primer on the polyacrylate adhesive layer. After drying, a primer layer is obtained on the polyacrylate adhesive layer.

[0053] Specifically, the mixture is dried with air at room temperature for 2 to 3 minutes.

[0054] S4, coating the silicone adhesive on the release film, and heating and drying to form a silicone adhesive layer on the release film.

[0055] Specifically, the heating and drying temperature is 100 to 180° C., and the drying time is 2 to 5 minutes.

[0056] S5. Laminating the silicone adhesive layer and the primer layer to obtain a substrate-free adhesive film.

[0057] The substrate-free adhesive film and its preparation process of the present invention will be described in detail below with reference to specific examples and comparative examples.

[0058] Example 1

[0059] (1) 8 parts of acrylic modified silicone resin (Si Hai SH-656874), 8 parts of polymethyl hydrogen siloxane, 5 parts of γ-(2,3-epoxypropoxy)propyl trimethoxysilane, 5 parts of γ-methacryloxypropyl trimethoxysilane, 5 parts of vinyl triethoxysilane and 50 parts of toluene are put into a reaction kettle, heated to 60-90° C. and stirred for 2-4 hours. After complete dissolution, 3 parts of tetrabutyl titanate and 2 parts of γ-isocyanate propyl triethoxysilane are added, and the mixture is stirred for another 2 hours under heat preservation conditions until it is evenly mixed, and then sealed and stored for later use;

[0060] (2) coating a high release force release film (Jinghua JTPT50D-R4 single-sided release film) with polyacrylic acid glue (Jinghua W-983 high viscosity glue) and drying it in an oven at 70-110° C. for 3-5 minutes to obtain a polyacrylate adhesive layer with a thickness of 50-55 μm;

[0061] (3) spraying a layer of primer on the surface of the dried polyacrylate adhesive layer, and blowing air at room temperature for 2-3 minutes to form a primer layer on the polyacrylate adhesive layer, the primer layer thickness of which is 3-5 μm;

[0062] (4) Coating a fluoroplastic release film (original color F5010) with silicone glue (Jinghua SO-024 silicone glue) and baking in an oven at 100-180°C for 2-5 minutes to obtain a silicone adhesive layer with a thickness of 30-35 μm;

[0063] (5) The dried silicone adhesive layer and the polyacrylate adhesive layer coated with a primer layer prepared in (3) are sandwiched and rolled up to obtain the substrate-free adhesive film of the present invention.

[0064] Example 2

[0065] (1) 10 parts of acrylic modified silicone resin (Si Hai SH-656874), 12 parts of polymethyl hydrogen siloxane, 7 parts of γ-(2,3-epoxypropoxy)propyl trimethoxysilane, 8 parts of γ-methacryloxypropyl trimethoxysilane, 7 parts of vinyl triethoxysilane and 60 parts of ethyl acetate were added into a reaction kettle, heated to 60-90° C. and stirred for 2-4 hours. After complete dissolution, 5 parts of tetrabutyl titanate and 5 parts of γ-isocyanate propyl triethoxysilane were added, and the mixture was stirred for another 2 hours under heat preservation conditions until uniform mixing was achieved. The mixture was then sealed and stored for later use.

[0066] (2) Applying polyacrylic acid glue (Jinghua W-983 high viscosity glue) on a high release force release film (Jinghua JTPT50D-R4 single-sided release film) and drying in an oven at 70-110° C. for 3-5 minutes to obtain a polyacrylic acid ester adhesive layer with a thickness of 30-35 μm;

[0067] (3) spraying a layer of primer on the surface of the dried polyacrylate adhesive layer, and blowing air at room temperature for 2-3 minutes to form a primer layer on the polyacrylate adhesive layer, the primer layer thickness of which is 3-5 μm;

[0068] (4) Coating a fluoroplastic release film (original color F5010) with silicone glue (Jinghua SO-024 silicone glue) and baking in an oven at 100-180°C for 2-5 minutes to obtain a silicone adhesive layer with a thickness of 30-35 μm;

[0069] (5) The dried silicone adhesive layer and the polyacrylate adhesive layer coated with a primer layer prepared in (3) are sandwiched and rolled up to obtain the substrate-free adhesive film of the present invention.

[0070] Example 3

[0071] (1) Add 5 parts of acrylic modified silicone resin (Si Hai SH-656874), 6 parts of polymethyl hydrogen siloxane, 3 parts of γ-(2,3-epoxypropoxy)propyl trimethoxysilane, 3 parts of γ-methacryloxypropyl trimethoxysilane, 4 parts of vinyl triethoxysilane and 30-60 parts of ethyl acetate into a reaction kettle, heat to 60-90° C. and stir for 2-4 hours, add 3 parts of tetrabutyl titanate and 2 parts of γ-isocyanate propyl triethoxysilane after they are completely dissolved, continue stirring for 2 hours under heat preservation conditions to mix evenly, and then seal and store for later use;

[0072] (2) Applying polyacrylic acid glue (Jinghua W-983 high viscosity glue) on a high release force release film (Jinghua JTPT50D-R4 single-sided release film) and drying in an oven at 70-110° C. for 3-5 minutes to obtain a polyacrylic acid ester adhesive layer with a thickness of 30-35 μm;

[0073] (3) spraying a layer of primer on the surface of the dried polyacrylate adhesive layer, and blowing air at room temperature for 2-3 minutes to form a primer layer on the polyacrylate adhesive layer, the primer layer thickness of which is 3-5 μm;

[0074] (4) Coating a fluoroplastic release film (original color F5010) with silicone glue (Jinghua SO-024 silicone glue) and baking in an oven at 100-180°C for 2-5 minutes to obtain a silicone adhesive layer with a thickness of 30-35 μm;

[0075] (5) The dried silicone adhesive layer and the polyacrylate adhesive layer coated with a primer layer prepared in (3) are sandwiched and rolled up to obtain the substrate-free adhesive film of the present invention.

[0076] Example 4

[0077] (1) 10 parts of acrylic modified silicone resin (Si Hai SH-656874), 6 parts of polymethyl hydrogen siloxane, 4 parts of γ-(2,3-epoxypropoxy)propyl trimethoxy silane, 6 parts of γ-methacryloxypropyl trimethoxy silane, 5 parts of vinyl triethoxy silane and 50 parts of toluene are put into a reaction kettle, heated to 60-90°C and stirred for 2-4 hours, and after complete dissolution, 5 parts of tetrabutyl titanate and 4 parts of γ-isocyanate propyl triethoxy silane are added, and the mixture is stirred for another 2 hours under heat preservation conditions until it is evenly mixed, and then sealed and stored for later use;

[0078] (2) coating a polyacrylic acid glue (Jinghua W-983 high viscosity glue) on a high release force release film (Jinghua JTPT50D-R4 single-sided release film) and drying it in an oven at 70-110° C. for 5-10 minutes to obtain a polyacrylate adhesive layer with a thickness of 100-110 μm;

[0079] (3) spraying a layer of primer on the surface of the dried polyacrylate adhesive layer, and blowing air at room temperature for 2-3 minutes to form a primer layer on the polyacrylate adhesive layer, the primer layer thickness of which is 3-5 μm;

[0080] (4) Coating a fluoroplastic release film (original color F5010) with silicone glue (Jinghua SO-024 silicone glue) and baking in an oven at 100-180°C for 2-5 minutes to obtain a silicone adhesive layer with a thickness of 30-35 μm;

[0081] (5) The dried silicone adhesive layer and the polyacrylate adhesive layer coated with a primer layer prepared in (3) are sandwiched and rolled up to obtain the substrate-free adhesive film of the present invention.

[0082] Comparative Example 1

[0083] (1) Add 5-10 parts of acrylic modified silicone resin (Si Hai SH-656874), 1 part of polymethyl hydrogen siloxane, and 30-60 parts of diluent into a reaction kettle, heat to 60-90°C and stir for 2-4 hours. After complete dissolution, continue stirring for another 2 hours under heat preservation conditions to mix evenly, and then seal and store for later use;

[0084] (2) Applying polyacrylic acid glue (Jinghua W-983 high viscosity glue) on a high release force release film (Jinghua JTPT50D-R4 single-sided release film) and drying in an oven at 70-110° C. for 3-5 minutes to obtain a polyacrylic acid ester adhesive layer with a thickness of 30-35 μm;

[0085] (3) spraying a layer of primer on the surface of the dried polyacrylate adhesive layer, and blowing air at room temperature for 2-3 minutes to form a primer layer on the polyacrylate adhesive layer, the primer layer thickness of which is 3-5 μm;

[0086] (4) Coating a fluoroplastic release film (original color F5010) with silicone glue (Jinghua SO-024 silicone glue) and baking in an oven at 100-180°C for 2-5 minutes to obtain a silicone adhesive layer with a thickness of 30-35 μm;

[0087] (5) The dried silicone adhesive layer and the polyacrylate adhesive layer coated with a primer layer prepared in (3) are sandwiched and rolled up to obtain the substrate-free adhesive film of the present invention.

[0088] Comparative Example 2

[0089] (1) Applying polyacrylic acid glue (Jinghua W-983 high viscosity glue) on a high release force release film (Jinghua JTPT50D-R4 single-sided release film) and drying in an oven at 70-110° C. for 3-5 minutes to obtain a polyacrylate adhesive layer with a thickness of 30-35 μm;

[0090] (2) The dried polyacrylate adhesive layer is bonded to one side of the 25uPET substrate;

[0091] (3) coating the other side of the substrate with silicone glue (Jinghua SO-024 silicone glue) and baking in an oven at 100-180° C. for 2-5 minutes to dry, thereby obtaining a silicone adhesive layer with a thickness of 30-35 μm;

[0092] (4) The dried silicone adhesive layer is laminated with a fluoroplastic release film and rolled up to obtain the substrate-free adhesive film of the present invention.

[0093] Comparative Example 3

[0094] (1) Applying polyacrylic acid glue (Jinghua W-983 high viscosity glue) on a high release force release film (Jinghua JTPT50D-R4 single-sided release film) and drying in an oven at 70-110° C. for 3-5 minutes to obtain a polyacrylate adhesive layer with a thickness of 30-35 μm;

[0095] (2) Coating a fluoroplastic release film (original color F5010) with silicone glue (Jinghua SO-024 silicone glue) and baking in an oven at 100-180°C for 2-5 minutes to obtain a silicone adhesive layer with a thickness of 30-35 μm;

[0096] (3) The dried silicone adhesive layer and the polyacrylate adhesive layer prepared in (1) are composited and then rolled up to obtain the substrate-free adhesive film of the present invention.

[0097] Comparative Example 4

[0098] (1) 2 parts of acrylic modified silicone resin (Si Hai SH-656874), 2 parts of polymethyl hydrogen siloxane, 10 parts of γ-(2,3-epoxypropoxy)propyl trimethoxysilane, 2 parts of γ-methacryloxypropyl trimethoxysilane, 2 parts of vinyl triethoxysilane and 50 parts of diluent are put into a reaction kettle, heated to 60-90°C and stirred for 2-4 hours, and after complete dissolution, 2 parts of tetrabutyl titanate and 2 parts of γ-isocyanate propyl triethoxysilane are added, and the mixture is stirred for another 2 hours under heat preservation conditions until it is evenly mixed, and then sealed and stored for later use;

[0099] (2) coating a high release force release film (Jinghua JTPT50D-R4 single-sided release film) with polyacrylic acid glue (Jinghua W-983 high viscosity glue) and drying it in an oven at 70-110° C. for 3-5 minutes to obtain a polyacrylate adhesive layer with a thickness of 50-55 μm;

[0100] (3) spraying a layer of primer on the surface of the dried polyacrylate adhesive layer, and blowing air at room temperature for 2-3 minutes to form a primer layer on the polyacrylate adhesive layer, the primer layer thickness of which is 3-5 μm;

[0101] (4) Coating a fluoroplastic release film (original color F5010) with silicone glue (Jinghua SO-024 silicone glue) and baking in an oven at 100-180°C for 2-5 minutes to obtain a silicone adhesive layer with a thickness of 30-35 μm;

[0102] (5) The dried silicone adhesive layer and the polyacrylate adhesive layer coated with a primer layer prepared in (3) are sandwiched and rolled up to obtain the substrate-free adhesive film of the present invention.

[0103] Comparative Example 5

[0104] (1) 15 parts of acrylic modified silicone resin (Si Hai SH-656874), 20 parts of polymethyl hydrogen siloxane, 5 parts of γ-(2,3-epoxypropoxy)propyl trimethoxysilane, 5 parts of γ-methacryloxypropyl trimethoxysilane, 5 parts of vinyl triethoxysilane and 50 parts of diluent are put into a reaction kettle, heated to 60-90°C and stirred for 2-4 hours, and after complete dissolution, 3 parts of tetrabutyl titanate and 2 parts of γ-isocyanate propyl triethoxysilane are added, and the mixture is stirred for another 2 hours under heat preservation conditions until it is evenly mixed, and then sealed and stored for later use;

[0105] (2) coating a high release force release film (Jinghua JTPT50D-R4 single-sided release film) with polyacrylic acid glue (Jinghua W-983 high viscosity glue) and drying it in an oven at 70-110° C. for 3-5 minutes to obtain a polyacrylate adhesive layer with a thickness of 50-55 μm;

[0106] (3) spraying a layer of primer on the surface of the dried polyacrylate adhesive layer, and blowing air at room temperature for 2-3 minutes to form a primer layer on the polyacrylate adhesive layer, the primer layer thickness of which is 3-5 μm;

[0107] (4) Coating a fluoroplastic release film (original color F5010) with silicone glue (Jinghua SO-024 silicone glue) and baking in an oven at 100-180°C for 2-5 minutes to obtain a silicone adhesive layer with a thickness of 30-35 μm;

[0108] (5) The dried silicone adhesive layer and the polyacrylate adhesive layer coated with a primer layer prepared in (3) are sandwiched and rolled up to obtain the substrate-free adhesive film of the present invention.

[0109] The performance tests were performed on the films in Examples 1 to 4 and Comparative Examples 1 to 5, and the data shown in the following table were obtained.

[0110]

[0111]

[0112] Note: Composite silicone foam bending test method: Step 1: Compound the silicone adhesive layer of the substrate-free film to the silicone foam surface; Step 2: Cut the compounded sample into strips of 20cm in length and 20mm in width; Step 3: Overlap the two ends of the cut strips along the length direction and fix them with 20mm wide tape; Bend the middle part of the strip, leave it for 72 hours and observe the separation of the glue and foam.

[0113] From the description of the bending performance after laminating the silicone foam in the above table, it can be clearly seen that the substrate-free adhesive film of the present invention and the silicone foam are not separated; while the adhesive films and silicone foams in Comparative Examples 1 to 5 are partially separated.

[0114] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.

[0115] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A substrate-free adhesive film, characterized in that: The invention comprises a laminated silicone adhesive layer, a primer layer and a polyacrylate adhesive layer; the primer layer comprises the following raw material components by weight: 10 to 22 parts of a film former, 11 to 26 parts of a coupling agent, 5 to 10 parts of a catalyst and 30 to 60 parts of a diluent.

2. The substrate-free adhesive film according to claim 1, characterized in that: The film-forming agent comprises acrylic modified silicone resin and polymethyl hydrogen siloxane, and the mass ratio of the acrylic modified silicone resin to the polymethyl hydrogen siloxane is (5-10): (5-12).

3. The substrate-free adhesive film according to claim 1, characterized in that: The coupling agent includes γ-(2,3-epoxypropoxy)propyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane and vinyltriethoxysilane, and the mass ratio of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane and vinyltriethoxysilane is (3-8): (3-10): (5-8).

4. The substrate-free adhesive film according to claim 1, characterized in that: The catalyst comprises tetrabutyl titanate and γ-isocyanate propyltriethoxysilane, and the mass ratio of the tetrabutyl titanate to the γ-isocyanate propyltriethoxysilane is (3-5): (2-5).

5. The substrate-free adhesive film according to claim 1, characterized in that: The diluent includes at least one of toluene, ethyl acetate, butanone and solvent oil.

6. The substrate-free adhesive film according to claim 1, characterized in that: The primer layer comprises the following raw material components by weight: 5-10 parts of acrylic modified silicone resin, 5-12 parts of polymethyl hydrogen siloxane, 3-8 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, 3-10 parts of γ-methacryloxypropyltrimethoxysilane, 5-8 parts of vinyltriethoxysilane, 3-5 parts of tetrabutyl titanate, 2-5 parts of γ-isocyanatepropyltriethoxysilane, and 30-60 parts of diluent.

7. The substrate-free adhesive film according to claim 1, characterized in that: The substrate-free adhesive film further comprises a fluoroplastic release film, and the fluoroplastic release film is attached to the side of the silicone adhesive layer that is away from the primer layer.

8. The substrate-free adhesive film according to claim 1, characterized in that: The substrate-free adhesive film further comprises a high-release-force release film, which is attached to a side of the polyacrylate adhesive layer that is away from the primer layer.

9. The substrate-free adhesive film according to claim 1, characterized in that: The thickness of the substrate-free adhesive film is 30 to 300 μm, and the tensile strength of the substrate-free adhesive film is greater than 2 MPa; The thickness of the silicone adhesive layer is 5 to 50 μm; The thickness of the polyacrylate adhesive layer is 20 to 200 μm.

10. A process for preparing a substrate-free adhesive film according to any one of claims 1 to 9, characterized in that: The following steps are involved: The film-forming agent, coupling agent and diluent in the raw materials of the primer layer are mixed in proportion, heated and mixed evenly, and then a catalyst is added to obtain a primer after reaction; Applying polyacrylate adhesive on the release film, and forming a polyacrylate adhesive layer on the release film after heating and drying; A layer of primer is sprayed on the polyacrylate adhesive layer, and after drying, a primer layer is obtained on the polyacrylate adhesive layer; Applying silicone adhesive on the release film, and heating and drying to form a silicone adhesive layer on the release film; The silicone adhesive layer is laminated to the primer layer to obtain a substrate-free adhesive film.