Preparation method of low-volatility organic compound (VOCs) release and UV stripping sticker

Build double-arm dopamine and polymers through dopamine, combined with dynamic coordination UV tack reduction technology, solve the problems of limited use and VOCs release under wet conditions, achieving high viscosity, easy peeling and low toxicity, environmental protection sticker preparation.

CN118931419APending Publication Date: 2024-11-12RR DONNELLEY (GUANGDONG) PRINTING SOLUTIONS LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411251883.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing UV stripping stickers are limited in use under wet or water-containing conditions, and the hydrolysis of the binder components during UV irradiation leads to the release of VOCs, affecting environmental protection.

Method used

Dopamine is used to construct double-arm dopamine and dopamine polymers, adjust the stickiness of the sticker, and reduce the release of VOCs through dynamic coordination UV stickiness technology, achieving high initial viscosity and easy peeling effect of the sticker.

Benefits of technology

Stable use of stickers and low VOCs release under wet conditions are achieved, and toxicity and environmental impact are reduced through viscosine composed of bionic materials and water.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931419A_ABST
    Figure CN118931419A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a low-VOCs release and UV stripping sticker. The preparation method specifically comprises the following steps: step 1, preparing a dopamine monomer; step 2, preparing a dopamine polymer according to a product obtained in the step 1; step 3, preparing double-arm dopamine; step 4, preparing a UV dopamine adhesive according to products obtained in the step 2 and the step 3; step 5, preparing oligomer dopamine according to the product obtained in the step 1; and step 6, preparing the sticker according to products obtained in the step 4 and the step 5. According to the invention, dopamine is utilized to construct double-arm dopamine and a dopamine polymer, the viscosity of the sticker is adjusted, the initial viscosity strength of the sticker is high, and meanwhile, dynamic coordination UV viscosity reduction is adopted, so that the sticker is easy to peel, and the release of VOCs (Volatile Organic Compounds) is low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials and relates to a method for preparing a low VOCs release UV peeling sticker. Background Art

[0002] With the development of society, stickers are used more and more widely and are indispensable in daily life. As stickers, they need to have high viscosity in order to adhere firmly. However, the high viscosity of stickers will also bring a series of problems, such as the inability to quickly peel off the stickers after use. In order to solve this problem, people have developed heat-dispersible adhesives and UV peeling stickers. Up to now, the main principle of heat-dispersible adhesives is to add heat-expandable microspheres to the pressure-sensitive adhesive. The volume of the microspheres is expanded by heating to achieve physical isolation and reduce viscosity. UV peeling stickers are also called UV hydrolysis peeling stickers. The principle is that the polymer skeleton of the glue contains a large number of easily photodegradable functional groups, which undergo hydrolysis reaction when exposed to light. Compared with heat-dispersible adhesives, UV peeling stickers have certain advantages. For example, UV peeling stickers can be used in the field of temperature-sensitive materials, while heat-dispersible stickers cannot. Since UV peeling stickers currently use a hydrolysis peeling mechanism, the stickers have a greater impact on the environmental humidity and the dryness of the adhered objects, which limits their use under humid and water-containing conditions. At the same time, when UV is irradiated, the adhesive component in the sticker is hydrolyzed, resulting in the release of VOCs. Summary of the invention

[0003] The purpose of the present invention is to provide a preparation method of a low VOCs release, UV peelable sticker. The method uses dopamine to construct a double-arm dopamine and a dopamine polymer, adjusts the viscosity of the sticker, and achieves a high initial viscosity strength of the sticker. At the same time, dynamic coordination UV viscosity reduction is used to make the sticker easy to peel and have low VOCs release.

[0004] The technical solution adopted by the present invention is a method for preparing a low VOCs release, UV peelable sticker, which specifically comprises the following steps:

[0005] Step 1, preparing dopamine monomer;

[0006] Step 2, preparing a dopamine polymer according to the product obtained in step 1;

[0007] Step 3, preparing double-arm dopamine;

[0008] Step 4, preparing a UV dopamine adhesive according to the products obtained in step 2 and step 3;

[0009] Step 5, preparing oligomeric dopamine according to the product obtained in step 1;

[0010] Step 6, preparing a sticker according to the products obtained in steps 4 and 5.

[0011] The present invention is also characterized in that:

[0012] The specific process of step 1 is:

[0013] Take 5-10g of dopamine and dissolve it in 30-60mL of deionized water, add 0.1-0.2g of sodium borate and 0.15-0.3g of sodium carbonate, then add 8-16g of acrylic anhydride, set the reaction temperature to 45-60°C, react for 16-32h, cool to room temperature after the reaction, pour the reaction solution directly into 100-200mL of ice water, extract with 100-200mL of chloroform three times, combine the organic liquids, and collect the oily product dopamine monomer by rotary evaporation.

[0014] The specific process of step 2 is:

[0015] 3-6 g of dopamine monomer is dissolved in 10-20 mL of N,N-dimethylformamide solvent, and then 1-2 g of ethylene glycol methyl ether methacrylate is added, and then 10-30 mg of a catalyst is added, and the mixture is heated to 65-80° C. under nitrogen conditions for reaction for 16 hours. After the reaction is completed, a 7000-10000Da dialysis bag is used, and dialyzed in 100-200 mL of N,N-dimethylformamide and 100-200 mL of ethanol in turn, and the dialyzate is dried at 45-60° C. to obtain a powder product, namely, a dopamine polymer.

[0016] The specific process of step 3 is:

[0017] Take 5-10g dopamine and dissolve it in 15-30mL N-methylpyrrolidone, put the reaction solution into a 0°C ice water bath, add 7-14g isophorone diisocyanate under a nitrogen atmosphere, and react in the ice water bath for 1-2h; then increase the reaction temperature to 80-100°C and react for 8-16h, then add 7-14g isophorone diisocyanate, increase the reaction temperature to 120-140°C and continue to react for 4-8h; after the reaction is completed, cool to room temperature; pour the reaction solution directly into 100-200mL ice water, extract with 100-200mL chloroform three times, combine the organic liquids, and collect the oily product double-arm dopamine by rotary evaporation.

[0018] The specific process of step 4 is:

[0019] Step 4.1, dispersing 2-4 g of double-arm dopamine and 2-4 g of dopamine polymer in 4-6 mL of deionized water, and stirring at room temperature for 30-60 min to obtain a dopamine mixed solution;

[0020] Step 4.2, dissolve 1.2-2.4 g of FeCl3 in 4-6 mL of deionized water, and add it dropwise to the dopamine mixture through a dropping funnel, stirring while adding, with a stirring rate of 800-1000 r / min. After the addition is completed, add 0.8-1.6 g of triphenylsulfonium perfluorobutyl, stir at room temperature for 30-60 min, and obtain a UV dopamine adhesive.

[0021] The specific process of step 5 is:

[0022] Take 1-2g of dopamine monomer and dissolve it in 10-15mL of N,N-dimethylformamide solvent, then add 1-2g of diethylene glycol ethyl ether acrylate, 0.1-0.3g of ethylene glycol dimethacrylate, and then add 10-20mg of catalyst, heat to 65-80℃ under nitrogen conditions for reaction for 30-45min, and cool to room temperature after the reaction to obtain oligomer dopamine.

[0023] The catalysts in step 2 and step 5 are both azobisisobutyronitrile.

[0024] The specific process of step 6 is:

[0025] Take 5cmx10cm label paper, apply oligomer dopamine on the surface of the label paper by screen printing, with a coating thickness of 10-20um, irradiate the coated label with ultraviolet light for 10-20s, bake in an oven at 45°C for 12-18h, and print a layer of UV dopamine adhesive on the side of the sticker coated with oligomer dopamine by screen printing, with a coating thickness of 30-50um, to obtain a sticker with low VOCs release and UV peeling.

[0026] The beneficial effects of the present invention are as follows:

[0027] (1) The present invention uses UV light to release acid conditions to achieve dynamic coordination of the double-arm dopamine adhesive to achieve the effect of reducing viscosity and easy peeling. In addition, the dopamine polymer adjusts the viscosity of the adhesive sticker. The solvent component in the sticker is water, which reduces the release of VOCs.

[0028] (2) The present invention uses dopamine to construct double-arm dopamine and dopamine polymers, adjusts the stickiness of the sticker, achieves high initial stickiness strength of the sticker, and uses dynamic coordination UV viscosity reduction. Therefore, the adhesive component is bionic material and water, which has the advantages of low toxicity, green environmental protection, and low VOCs release. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a sticker model diagram of Example 1 of the preparation method of the low VOCs release, UV peeling sticker of the present invention and Comparative Examples 1, 3, 4 and 5. DETAILED DESCRIPTION

[0030] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0031] The method for preparing the low VOCs release UV peeling sticker of the present invention specifically comprises the following steps:

[0032] Step 1, preparation of dopamine monomer, the specific process is as follows:

[0033] Take 5-10g of dopamine and dissolve it in 30-60mL of deionized water, add 0.1-0.2g of sodium borate and 0.15-0.3g of sodium carbonate. Then add 8-16g of acrylic anhydride. Set the reaction temperature to 45-60℃ and react for 16-32h. After the reaction is completed, cool to room temperature and pour the reaction solution directly into 100-200mL of 0℃ ice water. Repeat the 100-200mL chloroform extraction three times, combine the organic liquids, and collect the oily product dopamine monomer by rotary evaporation at 60-80℃.

[0034] Step 2, preparation of dopamine polymer, the specific process is as follows:

[0035] Take 3-6g of dopamine monomer and dissolve it in 10-20mL of N,N-dimethylformamide solvent, then add 1-2g of ethylene glycol methyl ether methacrylate, and then add 10-30mg of azobisisobutyronitrile catalyst. Heat to 65-80℃ under nitrogen and react for 16h. After the reaction, use a 7000-10000Da dialysis bag and dialyze in 100-200mL of N,N-dimethylformamide and 100-200mL of ethanol successively. The dialyzate is dried at 45-60℃ to obtain a powder product.

[0036] Step 3, preparation of double-arm dopamine, the specific process is as follows:

[0037] Take 5-10g dopamine and dissolve it in 15-30mL N-methylpyrrolidone, put the reaction solution in a 0℃ ice-water bath, add 7-14g isophorone diisocyanate under nitrogen atmosphere, and react in an ice-water bath for 1-2h. Then increase the reaction temperature to 80-100℃ and react for 8-16h, then add 7-14g isophorone diisocyanate, increase the reaction temperature to 120-140℃ and continue to react for 4-8h. After the reaction is completed, cool to room temperature. Pour the reaction solution directly into 100-200mL of 0℃ ice water, repeat 100-200mL chloroform extraction three times, combine the organic liquid, and collect the oily product double-arm dopamine by rotary evaporation at 60℃.

[0038] Step 4, preparation of UV dopamine adhesive, the specific process is as follows:

[0039] Disperse 2-4g of double-arm dopamine and 2-4g of dopamine polymer in 4-6mL of deionized water and stir at room temperature for 30-60min to obtain a dopamine mixed solution. Then dissolve 1.2-2.4g of FeCl3 in 4-6mL of deionized water and slowly add it to the dopamine mixed solution through a dropping funnel (addition time is 10-15min), and stir rapidly (800-1000r / min) while adding. After the addition is completed, add 0.8-1.6g of triphenylsulfonium perfluorobutyl and stir at room temperature for 30-60min.

[0040] Step 5, preparation of oligomer dopamine, the specific process is as follows:

[0041] Take 1-2g of dopamine monomer and dissolve it in 10-15mL of N,N-dimethylformamide solvent, then add 1-2g of diethylene glycol ethyl ether acrylate, 0.1-0.3g of ethylene glycol dimethacrylate, and then add 10-20mg of azobisisobutyronitrile catalyst. Heat to 65-80℃ under nitrogen for 30-45min, and cool to room temperature after the reaction to obtain oligomer dopamine.

[0042] Step 6, preparation of low VOCs release, UV peeling sticker, the specific process is as follows:

[0043] Take 5cmx10cm label paper, apply oligomer dopamine on the surface of the label paper by screen printing, with a coating thickness of (10-20um), irradiate the coated label with a 45W UV lamp for 10-20s, and bake it in a 45℃ oven for 12-18h. On the side of the sticker coated with oligomer dopamine, print a layer of UV dopamine adhesive by screen printing, with a coating thickness of 30-50um, and the sticker is obtained.

[0044] Example 1

[0045] Step 1, preparation of dopamine monomer, the specific process is as follows:

[0046] Take 5g of dopamine and dissolve it in 30mL of deionized water, add 0.1g of sodium borate and 0.15g of sodium carbonate. Then add 8g of acrylic anhydride. The reaction temperature is set to 45℃ and the reaction is carried out for 16h. After the reaction is completed, cool to room temperature and pour the reaction solution directly into 100mL of ice water. Repeat the extraction with 100mL of chloroform three times, combine the organic liquids, and collect the oily product dopamine monomer by rotary evaporation at 60℃.

[0047] Step 2, preparation of dopamine polymer, the specific process is as follows:

[0048] Take 3g of dopamine monomer and dissolve it in 10mL of N,N-dimethylformamide solvent, then add 1g of ethylene glycol methyl ether methacrylate, and then add 10mg of azobisisobutyronitrile catalyst. Heat to 65℃ under nitrogen and react for 16h. After the reaction, use a 7000Da dialysis bag and dialyze in 100mL of N,N-dimethylformamide and 100mL of ethanol successively. The dialyzate is dried at 45℃ to obtain a powder product.

[0049] Step 3, preparation of double-arm dopamine, the specific process is as follows:

[0050] Take 5g dopamine and dissolve it in 15mL N-methylpyrrolidone, put the reaction solution in a 0℃ ice-water bath, add 7g isophorone diisocyanate under nitrogen atmosphere, and react in an ice-water bath for 1h. Then increase the reaction temperature to 80℃ for 8h, then add 7g isophorone diisocyanate, increase the reaction temperature to 120℃ and continue to react for 4h. After the reaction is completed, cool to room temperature. Pour the reaction directly into 100mL of 0℃ ice water, repeat 100mL chloroform extraction three times, combine the organic liquid, and collect the oily product double-arm dopamine by rotary evaporation at 60℃.

[0051] Step 4, preparation of UV dopamine adhesive, the specific process is as follows:

[0052] 2g of double-arm dopamine and 2g of dopamine polymer were dispersed in 4mL of deionized water and stirred at room temperature for 30min to obtain a dopamine mixed solution. Then 1.2g of FeCl3 was dissolved in 4mL of deionized water and slowly added to the dopamine mixed solution through a dropping funnel (addition time was 10min), with rapid stirring (800r / min) while adding. After the addition was completed, 0.8g of triphenylsulfonium perfluorobutyl was added and stirred at room temperature for 30min.

[0053] Step 5, preparation of oligomer dopamine, the specific process is as follows:

[0054] Take 1g of dopamine monomer and dissolve it in 10mL of N,N-dimethylformamide solvent, then add 1g of diethylene glycol ethyl ether acrylate, 0.1g of ethylene glycol dimethacrylate, and then add 10mg of azobisisobutyronitrile catalyst. Heat to 65℃ under nitrogen for 30min, and cool to room temperature after the reaction to obtain oligomer dopamine.

[0055] Step 6, preparation of low VOCs release, UV peeling sticker, the specific process is as follows:

[0056] Take a 5cmx10cm label base paper, and apply oligomer dopamine on the surface of the label paper by screen printing, with a coating thickness of (10um). The coated label is irradiated with a 45W ultraviolet lamp for 10s, and placed in a 45°C oven for 12h. After the sticker is coated with the oligomer dopamine layer, a layer of UV dopamine adhesive is further screen-printed with a coating thickness of 30um to obtain a sticker.

[0057] Comparative Example 1 (FeCl3 was not added to the UV dopamine adhesive, and the initial viscosity of the sticker was low)

[0058] Step 1, preparation of dopamine monomer, the specific process is as follows:

[0059] Take 5g of dopamine and dissolve it in 30mL of deionized water, add 0.1g of sodium borate and 0.15g of sodium carbonate. Then add 8g of acrylic anhydride. The reaction temperature is set to 45°C and the reaction is carried out for 16h. After the reaction is completed, cool to room temperature and pour the reaction solution directly into 100mL of ice water. Repeat the 100mL chloroform extraction three times, combine the organic liquids, and collect the oily product dopamine monomer by rotary evaporation.

[0060] Step 2, preparation of dopamine polymer, the specific process is as follows:

[0061] Take 3g of dopamine monomer and dissolve it in 10mL of N,N-dimethylformamide solvent, then add 1g of ethylene glycol methyl ether methacrylate, and then add 10mg of azobisisobutyronitrile catalyst. Heat to 65℃ under nitrogen and react for 16h. After the reaction, use a 7000Da dialysis bag and dialyze in 100mL of N,N-dimethylformamide and 100mL of ethanol successively. The dialyzate is dried at 45℃ to obtain a powder product.

[0062] Step 3, preparation of double-arm dopamine, the specific process is as follows:

[0063] Take 5g dopamine and dissolve it in 15mL N-methylpyrrolidone, put the reaction solution in a 0℃ ice-water bath, add 7g isophorone diisocyanate under nitrogen atmosphere, and react in an ice-water bath for 1h. Then increase the reaction temperature to 80℃ for 8h, then add 7g isophorone diisocyanate, increase the reaction temperature to 120℃ and continue to react for 4h. After the reaction is completed, cool to room temperature. Pour the reaction directly into 100mL of 0℃ ice water, repeat 100mL chloroform extraction three times, combine the organic liquid, and collect the oily product double-arm dopamine by rotary evaporation at 60℃.

[0064] Step 4, preparation of UV dopamine adhesive, the specific process is as follows:

[0065] 2g of double-arm dopamine and 2g of dopamine polymer were dispersed in 4mL of deionized water and stirred at room temperature for 30min to obtain a dopamine mixed solution. Then 4mL of deionized water was slowly added to the dopamine mixed solution through a dropping funnel (addition time was 10min), and the mixture was stirred rapidly (800r / min) while being added. After the addition was completed, 0.8g of triphenylsulfonium perfluorobutyl was added and stirred at room temperature for 30min.

[0066] Step 5, preparation of oligomer dopamine, the specific process is as follows:

[0067] Take 1g of dopamine monomer and dissolve it in 10mL of N,N-dimethylformamide solvent, then add 1g of diethylene glycol ethyl ether acrylate, 0.1g of ethylene glycol dimethacrylate, and then add 10mg of azobisisobutyronitrile catalyst. Heat to 65℃ under nitrogen for 30min, and cool to room temperature after the reaction to obtain oligomer dopamine.

[0068] Step 6, sticker preparation, the specific process is as follows:

[0069] Take a 5cmx10cm label base paper, and apply oligomer dopamine on the surface of the label paper by screen printing, with a coating thickness of (10um). The coated label is irradiated with a 45W ultraviolet lamp for 10s, and placed in a 45°C oven for 12h. After the sticker is coated with the oligomer dopamine layer, a layer of UV dopamine adhesive is further screen-printed with a coating thickness of 30um to obtain a sticker.

[0070] Comparative Example 2 (Triphenylsulfonium perfluorobutyl was not added to the UV dopamine adhesive, and no acid was released during UV irradiation, so viscosity reduction could not be achieved)

[0071] Step 1, preparation of dopamine monomer, the specific process is as follows:

[0072] Take 5g of dopamine and dissolve it in 30mL of deionized water, add 0.1g of sodium borate and 0.15g of sodium carbonate. Then add 8g of acrylic anhydride. The reaction temperature is set to 45°C and the reaction is carried out for 16h. After the reaction is completed, cool to room temperature and pour the reaction solution directly into 100mL of ice water. Repeat the 100mL chloroform extraction three times, combine the organic liquids, and collect the oily product dopamine monomer by rotary evaporation.

[0073] Step 2, preparation of dopamine polymer, the specific process is as follows:

[0074] Take 3g of dopamine monomer and dissolve it in 10mL of N,N-dimethylformamide solvent, then add 1g of ethylene glycol methyl ether methacrylate, and then add 10mg of azobisisobutyronitrile catalyst. Heat to 65℃ under nitrogen and react for 16h. After the reaction, use a 7000Da dialysis bag and dialyze in 100mL of N,N-dimethylformamide and 100mL of ethanol successively. The dialyzate is dried at 45℃ to obtain a powder product.

[0075] Step 3, preparation of double-arm dopamine, the specific process is as follows:

[0076] Take 5g dopamine and dissolve it in 15mL N-methylpyrrolidone, put the reaction solution in a 0℃ ice-water bath, add 7g isophorone diisocyanate under nitrogen atmosphere, and react in an ice-water bath for 1h. Then increase the reaction temperature to 80℃ for 8h, then add 7g isophorone diisocyanate, increase the reaction temperature to 120℃ and continue to react for 4h. After the reaction is completed, cool to room temperature. Pour the reaction directly into 100mL of 0℃ ice water, repeat 100mL chloroform extraction three times, combine the organic liquid, and collect the oily product double-arm dopamine by rotary evaporation at 60℃.

[0077] Step 4, preparation of UV dopamine adhesive, the specific process is as follows:

[0078] 2 g of double-arm dopamine and 2 g of dopamine polymer were dispersed in 4 mL of deionized water and stirred at room temperature for 30 min to obtain a dopamine mixed solution. Then 1.2 g of FeCl3 was dissolved in 4 mL of deionized water and slowly added to the dopamine mixed solution through a dropping funnel (addition time was 10 min), and the mixture was rapidly stirred (800 r / min) while being added, and a UV dopamine adhesive was obtained after the addition was completed.

[0079] Step 5, preparation of oligomer dopamine, the specific process is as follows:

[0080] Take 1g of dopamine monomer and dissolve it in 10mL of N,N-dimethylformamide solvent, then add 1g of diethylene glycol ethyl ether acrylate, 0.1g of ethylene glycol dimethacrylate, and then add 10mg of azobisisobutyronitrile catalyst. Heat to 65℃ under nitrogen for 30min, and cool to room temperature after the reaction to obtain oligomer dopamine.

[0081] Step 6, sticker preparation, the specific process is as follows:

[0082] Take a 5cmx10cm label base paper, and apply oligomer dopamine on the surface of the label paper by screen printing, with a coating thickness of (10um). The coated label is irradiated with a 45W ultraviolet lamp for 10s, and placed in a 45°C oven for 12h. After the sticker is coated with the oligomer dopamine layer, a layer of UV dopamine adhesive is further screen-printed with a coating thickness of 30um to obtain a sticker.

[0083] Comparative Example 3 (no oligomer dopamine layer was applied to the sticker, and adhesive residue remained when the sticker was peeled off after UV irradiation)

[0084] Step 1, preparation of dopamine monomer, the specific process is as follows:

[0085] Take 5g of dopamine and dissolve it in 30mL of deionized water, add 0.1g of sodium borate and 0.15g of sodium carbonate. Then add 8g of acrylic anhydride. The reaction temperature is set to 45°C and the reaction is carried out for 16h. After the reaction is completed, cool to room temperature and pour the reaction solution directly into 100mL of ice water. Repeat the 100mL chloroform extraction three times, combine the organic liquids, and collect the oily product dopamine monomer by rotary evaporation.

[0086] Step 2, preparation of dopamine polymer, the specific process is as follows:

[0087] Take 3g of dopamine monomer and dissolve it in 10mL of N,N-dimethylformamide solvent, then add 1g of ethylene glycol methyl ether methacrylate, and then add 10mg of azobisisobutyronitrile catalyst. Heat to 65℃ under nitrogen and react for 16h. After the reaction, use a 7000Da dialysis bag and dialyze in 100mL of N,N-dimethylformamide and 100mL of ethanol successively. The dialyzate is dried at 45℃ to obtain a powder product.

[0088] Step 3, preparation of double-arm dopamine, the specific process is as follows:

[0089] Take 5g dopamine and dissolve it in 15mL N-methylpyrrolidone, put the reaction solution in a 0℃ ice-water bath, add 7g isophorone diisocyanate under nitrogen atmosphere, and react in an ice-water bath for 1h. Then increase the reaction temperature to 80℃ for 8h, then add 7g isophorone diisocyanate, increase the reaction temperature to 120℃ and continue to react for 4h. After the reaction is completed, cool to room temperature. Pour the reaction directly into 100mL of 0℃ ice water, repeat 100mL chloroform extraction three times, combine the organic liquid, and collect the oily product double-arm dopamine by rotary evaporation at 60℃.

[0090] Step 4, preparation of UV dopamine adhesive, the specific process is as follows:

[0091] 2g of double-arm dopamine and 2g of dopamine polymer were dispersed in 4mL of deionized water and stirred at room temperature for 30min to obtain a dopamine mixed solution. Then 1.2g of FeCl3 was dissolved in 4mL of deionized water and slowly added to the dopamine mixed solution through a dropping funnel (addition time was 10min), with rapid stirring (800r / min) while adding. After the addition was completed, 0.8g of triphenylsulfonium perfluorobutyl was added and stirred at room temperature for 30min.

[0092] Step 5, sticker preparation, the specific process is as follows:

[0093] Take a 5cmx10cm label paper and screen print a layer of UV dopamine adhesive on the upper surface of the sticker with a coating thickness of 30um.

[0094] Comparative Example 4 (dopamine polymer replaced with acrylic polymer, low initial viscosity, poor viscosity reduction effect, glue residue and VOCss release)

[0095] Step 1, preparation of acrylic acid ester polymer, the specific process is:

[0096] Take 3g of methyl acrylate and dissolve it in 10mL of N,N-dimethylformamide solvent, then add 1g of ethylene glycol methyl ether methacrylate, and then add 10mg of azobisisobutyronitrile catalyst. Heat to 65℃ under nitrogen and react for 16h. After the reaction, use a 7000Da dialysis bag and dialyze in 100mL of N,N-dimethylformamide and 100mL of ethanol successively. The dialyzate is dried at 45℃ to obtain a powder product.

[0097] Step 2, preparation of double-arm dopamine, the specific process is:

[0098] Take 5g dopamine and dissolve it in 15mL N-methylpyrrolidone, put the reaction solution in a 0℃ ice-water bath, add 7g isophorone diisocyanate under nitrogen atmosphere, and react in an ice-water bath for 1h. Then increase the reaction temperature to 80℃ for 8h, then add 7g isophorone diisocyanate, increase the reaction temperature to 120℃ and continue to react for 4h. After the reaction is completed, cool to room temperature. Pour the reaction directly into 100mL of 0℃ ice water, repeat 100mL chloroform extraction three times, combine the organic liquid, and collect the oily product double-arm dopamine by rotary evaporation at 60℃.

[0099] Step 3, preparation of UV dopamine adhesive, the specific process is:

[0100] 2g of double-arm dopamine and 2g of acrylic polymer were dispersed in 4mL of deionized water and stirred at room temperature for 30min to obtain a dopamine mixed solution. Then 1.2g of FeCl3 was dissolved in 4mL of deionized water and slowly added to the dopamine mixed solution through a dropping funnel (addition time was 10min), with rapid stirring (800r / min) while adding. After the addition was completed, 0.8g of triphenylsulfonium perfluorobutyl was added and stirred at room temperature for 30min.

[0101] Step 4, preparation of oligomer dopamine, the specific process is:

[0102] Take 1g of dopamine monomer and dissolve it in 10mL of N,N-dimethylformamide solvent, then add 1g of diethylene glycol ethyl ether acrylate, 0.1g of ethylene glycol dimethacrylate, and then add 10mg of azobisisobutyronitrile catalyst. Heat to 65℃ under nitrogen for 30min, and cool to room temperature after the reaction to obtain oligomer dopamine.

[0103] step

[0104] Step 5, sticker preparation, the specific process is:

[0105] Take 5cmx10cm label paper, apply oligomer dopamine on the label paper surface by screen printing, the coating thickness is (10um), the coated label is irradiated with 45W UV lamp for 10s, and baked in 45℃ oven for 12h. A layer of UV dopamine adhesive is further applied by screen printing on the sticker coated with oligomer dopamine layer, the coating thickness is 30um.

[0106] Comparative Example 5 (no double-arm dopamine was added to the UV dopamine adhesive, low initial viscosity and poor viscosity reduction effect)

[0107] Step 1, preparation of dopamine monomer, specifically:

[0108] Take 5g of dopamine and dissolve it in 30mL of deionized water, add 0.1g of sodium borate and 0.15g of sodium carbonate. Then add 8g of acrylic anhydride. The reaction temperature is set to 45℃ and the reaction is carried out for 16h. After the reaction is completed, cool to room temperature and pour the reaction solution directly into 100mL of 0℃ ice water. Repeat the 1000mL chloroform extraction three times, combine the organic liquids, and collect the oily product dopamine monomer by rotary evaporation at 60℃.

[0109] Step 2, preparation of dopamine polymer, specifically:

[0110] Take 3g of dopamine monomer and dissolve it in 10mL of N,N-dimethylformamide solvent, then add 1g of ethylene glycol methyl ether methacrylate, and then add 10mg of azobisisobutyronitrile catalyst. Heat to 65℃ under nitrogen and react for 16h. After the reaction, use a 7000Da dialysis bag and dialyze in 100mL of N,N-dimethylformamide and 100mL of ethanol successively. The dialyzate is dried at 45℃ to obtain a powder product.

[0111] Step 3, preparation of UV dopamine adhesive, the specific process is:

[0112] Disperse 2g of dopamine polymer in 4mL of deionized water and stir at room temperature for 30min to obtain a dopamine mixed solution. Then dissolve 1.2g of FeCl3 in 4mL of deionized water and slowly add it to the dopamine mixed solution through a dropping funnel (addition time is 10min), stirring rapidly (800r / min) while adding. After the addition is completed, add 0.8g of triphenylsulfonium perfluorobutyl and stir at room temperature for 30min.

[0113] Step 4, preparation of oligomer dopamine, the specific process is:

[0114] Take 1g of dopamine monomer and dissolve it in 10mL of N,N-dimethylformamide solvent, then add 1g of diethylene glycol ethyl ether acrylate, 0.1g of ethylene glycol dimethacrylate, and then add 10mg of azobisisobutyronitrile catalyst. Heat to 65℃ under nitrogen for 30min, and cool to room temperature after the reaction to obtain oligomer dopamine.

[0115] Step 5, sticker preparation, the specific process is:

[0116] Take 5cmx10cm label paper, apply oligomer dopamine on the label paper surface by screen printing, the coating thickness is (10um), the coated label is irradiated with 45W UV lamp for 10s, and baked in 45℃ oven for 12h. A layer of UV dopamine adhesive is further applied by screen printing on the sticker coated with oligomer dopamine layer, the coating thickness is 30um.

[0117] Experimental Results

[0118]

[0119] The peel strength is tested using the standard method of GB / T 2792-2014, and the VOCs test method is the standard test method of GB18583-2008. The peel strength of the sticker is tested on the surface of the steel plate.

[0120] In Example 1, the initial peeling force of the sticker was 20N / 25mm, but after UV irradiation, the peeling force decreased to 5N / 25mm, as shown in Table 1. The main reason is that when the triphenylsulfonium perfluorobutyl acid release agent is exposed to light, the acid released causes dopamine to react with Fe 3+ The formed coordination bonds are destroyed.

[0121] In comparative example 1, FeCl3 was not added to the UV dopamine adhesive, and the viscosity of the sticker remained almost unchanged before and after UV irradiation, and was relatively low. The main reason is that the dopamine polymer and the two-arm dopamine cannot form a coordination bond (such as Figure 1 In Example 1 and Comparative Example 1), the coordination polymer cannot be formed and the initial viscosity is low. In addition, it cannot be irradiated with UV and has no effect on acid.

[0122] In the comparative example 2 UV dopamine adhesive, triphenylsulfonium perfluorobutyl was not added. Although it had strong peeling force before UV irradiation, the triphenylsulfonium perfluorobutyl component did not release acid during UV irradiation, so it could not reduce viscosity.

[0123] In Comparative Example 3, the sticker was not coated with an oligomer dopamine layer. When the sticker was peeled off after UV irradiation, there was adhesive residue. This is because the sticker surface was not treated with oligomer dopamine. The UV dopamine adhesive was directly coated on the sticker surface (such as Figure 1 In comparative example 3), the adhesion between them is poor, resulting in residues when peeled off.

[0124] In Comparative Example 4, the dopamine polymer was replaced with an acrylate polymer. The acrylate polymer component and the two-arm dopamine failed to form a coordination bond crosslink, resulting in low peel strength before UV irradiation. Compared with Example 1, Comparative Example 4 lacks a dopamine polymer component, and the coordination bonds formed are small, resulting in poor viscosity reduction effect. In addition, the acrylate polymer and the oligomer dopamine layer cannot form an interaction force (such as Figure 1 Comparative Example 4) has adhesive residue when peeled off. In Comparative Example 4, pure organic methyl acrylate monomer is used, resulting in VOCss release.

[0125] In the comparative example 5 sticker, the UV dopamine adhesive was not added with double-arm dopamine, Fe 3+ It can coordinate with double-arm dopamine and dopamine polymer to form a three-dimensional network structure, thereby improving the adhesive viscosity. Therefore, the lack of double-arm dopamine, the lack of the three-dimensional network structure of double-arm dopamine during peeling. At the same time, Fe 3+ The content of coordination bonds formed with dopamine is reduced (such as Figure 1 Comparative Example 5) has poor viscosity reduction effect.

[0126] Example 2

[0127] Step 1, preparation of dopamine monomer, the specific process is as follows:

[0128] Take 8g of dopamine and dissolve it in 40mL of deionized water, add 0.15g of sodium borate and 0.2g of sodium carbonate. Then add 12g of acrylic anhydride. The reaction temperature is set to 55°C and the reaction is carried out for 24h. After the reaction is completed, cool to room temperature and pour the reaction solution directly into 150mL of ice water. Repeat the extraction with 150mL of chloroform three times, combine the organic liquids, and collect the oily product dopamine monomer by rotary evaporation at 70°C.

[0129] Step 2, preparation of dopamine polymer, the specific process is as follows:

[0130] Take 4g of dopamine monomer and dissolve it in 15mL of N,N-dimethylformamide solvent, then add 1.5g of ethylene glycol methyl ether methacrylate, and then add 20mg of azobisisobutyronitrile catalyst. Heat to 75℃ under nitrogen and react for 16h. After the reaction, use 8000Da dialysis bag and dialyze in 150mL of N,N-dimethylformamide and 150mL of ethanol successively. The dialyzate is dried at 55℃ to obtain a powder product.

[0131] Step 3, preparation of double-arm dopamine, the specific process is as follows:

[0132] Take 8g of dopamine and dissolve it in 20mL of N-methylpyrrolidone. Put the reaction solution in a 0℃ ice-water bath. Add 9g of isophorone diisocyanate under a nitrogen atmosphere and react in an ice-water bath for 1.5h. Then increase the reaction temperature to 90℃ for 12h, then add 9g of isophorone diisocyanate, increase the reaction temperature to 130℃ and continue to react for 7h. After the reaction is completed, cool to room temperature. Pour the reaction directly into 150mL of 0℃ ice water, extract with 150mL of chloroform three times, combine the organic liquid, and collect the oily product double-arm dopamine by rotary evaporation at 60℃.

[0133] Step 4, preparation of UV dopamine adhesive, the specific process is as follows:

[0134] 3g of double-arm dopamine and 3g of dopamine polymer were dispersed in 5mL of deionized water and stirred at room temperature for 50min to obtain a dopamine mixed solution. Then 1.8g of FeCl3 was dissolved in 5mL of deionized water and slowly added to the dopamine mixed solution through a dropping funnel (addition time was 12min), with rapid stirring (900r / min) while adding. After the addition was completed, 1.2g of triphenylsulfonium perfluorobutyl was added and stirred at room temperature for 40min.

[0135] Step 5, preparation of oligomer dopamine, the specific process is as follows:

[0136] 1.5 g of dopamine monomer was dissolved in 12 mL of N,N-dimethylformamide solvent, and then 1.5 g of diethylene glycol ethyl ether acrylate, 0.2 g of ethylene glycol dimethacrylate, and then 15 mg of azobisisobutyronitrile catalyst were added. The mixture was heated to 75°C under nitrogen and reacted for 40 min. After the reaction was completed, the mixture was cooled to room temperature to obtain oligomeric dopamine.

[0137] Step 6, preparation of low VOCs release, UV peeling sticker, the specific process is as follows:

[0138] Take a 5cmx10cm label base paper, and apply oligomer dopamine on the surface of the label paper by screen printing, with a coating thickness of (15um). The coated label is irradiated with a 45W ultraviolet lamp for 15s, and placed in a 45°C oven for 16h. After the sticker is coated with the oligomer dopamine layer, a layer of UV dopamine adhesive is further screen-printed with a coating thickness of 40um to obtain a sticker.

[0139] Example 3

[0140] Step 1, preparation of dopamine monomer, the specific process is as follows:

[0141] Take 10g of dopamine and dissolve it in 60mL of deionized water, add 0.2g of sodium borate and 0.3g of sodium carbonate. Then add 16g of acrylic anhydride. The reaction temperature is set to 60℃ and the reaction is carried out for 32h. After the reaction is completed, cool to room temperature and pour the reaction solution directly into 200mL of ice water. Repeat the extraction with 200mL of chloroform three times, combine the organic liquids, and collect the oily product dopamine monomer by rotary evaporation at 80℃.

[0142] Step 2, preparation of dopamine polymer, the specific process is as follows:

[0143] Take 6g of dopamine monomer and dissolve it in 20mL of N,N-dimethylformamide solvent, then add 2g of ethylene glycol methyl ether methacrylate, and then add 30mg of azobisisobutyronitrile catalyst. Heat to 80℃ under nitrogen and react for 16h. After the reaction, use a 10000Da dialysis bag and dialyze in 200mL of N,N-dimethylformamide and 200mL of ethanol successively. The dialyzate is dried at 60℃ to obtain a powder product.

[0144] Step 3, preparation of double-arm dopamine, the specific process is as follows:

[0145] Take 10g dopamine and dissolve it in 30mL N-methylpyrrolidone, put the reaction solution in a 0℃ ice-water bath, add 14g isophorone diisocyanate under nitrogen atmosphere, and react in an ice-water bath for 2h. Then increase the reaction temperature to 100℃ and react for 16h, then add 14g isophorone diisocyanate, increase the reaction temperature to 140℃ and continue to react for 8h. After the reaction is completed, cool to room temperature. Pour the reaction directly into 200mL of 0℃ ice water, repeat 200mL chloroform extraction three times, combine the organic liquid, and collect the oily product double-arm dopamine by rotary evaporation at 60℃.

[0146] Step 4, preparation of UV dopamine adhesive, the specific process is as follows:

[0147] 4 g of double-arm dopamine and 4 g of dopamine polymer were dispersed in 6 mL of deionized water and stirred at room temperature for 60 min to obtain a dopamine mixed solution. Then 2.4 g of FeCl3 was dissolved in 6 mL of deionized water and slowly added to the dopamine mixed solution through a dropping funnel (addition time was 15 min), with rapid stirring (1000 r / min) while adding. After the addition was completed, 1.6 g of triphenylsulfonium perfluorobutyl was added and stirred at room temperature for 60 min.

[0148] Step 5, preparation of oligomer dopamine, the specific process is as follows:

[0149] Take 2g of dopamine monomer and dissolve it in 15mL of N,N-dimethylformamide solvent, then add 2g of diethylene glycol ethyl ether acrylate, 0.3g of ethylene glycol dimethacrylate, and then add 20mg of azobisisobutyronitrile catalyst. Heat to 80℃ under nitrogen for 45min, and cool to room temperature after the reaction to obtain oligomer dopamine.

[0150] Step 6, preparation of low VOCs release, UV peeling sticker, the specific process is as follows:

[0151] Take a 5cmx10cm label base paper, and apply oligomer dopamine on the surface of the label paper by screen printing, with a coating thickness of (20um). The coated label is irradiated with a 45W ultraviolet lamp for 20s, and placed in a 45°C oven for 18h. After the sticker is coated with the oligomer dopamine layer, a layer of UV dopamine adhesive is further screen-printed with a coating thickness of 50um to obtain a sticker.

Claims

1. A method for preparing a UV peelable sticker with low volatile organic compound (VOCs) release, Features: The specific steps include: Step 1, preparing dopamine monomer; Step 2, preparing a dopamine polymer according to the product obtained in step 1; Step 3, preparing double-arm dopamine; Step 4, preparing a UV dopamine adhesive according to the products obtained in step 2 and step 3; Step 5, preparing oligomeric dopamine according to the product obtained in step 1; Step 6, preparing a sticker according to the products obtained in steps 4 and 5.

2. A method for preparing a low volatile organic compound (VOCs) release, UV peelable sticker according to claim 1, Features: The specific process of step 1 is as follows: Take 5-10g of dopamine and dissolve it in 30-60mL of deionized water, add 0.1-0.2g of sodium borate and 0.15-0.3g of sodium carbonate, then add 8-16g of acrylic anhydride, set the reaction temperature to 45-60°C, react for 16-32h, cool to room temperature after the reaction, pour the reaction solution directly into 100-200mL of ice water, extract with 100-200mL of chloroform three times, combine the organic liquids, and collect the oily product dopamine monomer by rotary evaporation.

3. A method for preparing a low volatile organic compound (VOCs) release, UV peelable sticker according to claim 1, Features: The specific process of step 2 is: 3-6 g of dopamine monomer is dissolved in 10-20 mL of N,N-dimethylformamide solvent, and then 1-2 g of ethylene glycol methyl ether methacrylate is added, and then 10-30 mg of a catalyst is added, and the mixture is heated to 65-80° C. under nitrogen conditions for reaction for 16 hours. After the reaction is completed, a 7000-10000Da dialysis bag is used, and dialyzed in 100-200 mL of N,N-dimethylformamide and 100-200 mL of ethanol in turn, and the dialyzate is dried at 45-60° C. to obtain a powder product, namely, a dopamine polymer.

4. A method for preparing a low volatile organic compound (VOCs) release, UV peelable sticker according to claim 1, Features: The specific process of step 3 is as follows: Take 5-10g dopamine and dissolve it in 15-30mL N-methylpyrrolidone, put the reaction solution into a 0°C ice water bath, add 7-14g isophorone diisocyanate under a nitrogen atmosphere, and react in the ice water bath for 1-2h; then increase the reaction temperature to 80-100°C and react for 8-16h, then add 7-14g isophorone diisocyanate, increase the reaction temperature to 120-140°C and continue to react for 4-8h; after the reaction is completed, cool to room temperature; pour the reaction solution directly into 100-200mL ice water, extract with 100-200mL chloroform three times, combine the organic liquids, and collect the oily product double-arm dopamine by rotary evaporation.

5. A method for preparing a low volatile organic compound (VOCs) release, UV peelable sticker according to claim 1, Features: The specific process of step 4 is as follows: Step 4.1, dispersing 2-4 g of double-arm dopamine and 2-4 g of dopamine polymer in 4-6 mL of deionized water, and stirring at room temperature for 30-60 min to obtain a dopamine mixed solution; Step 4.2, add 1.2-2.4 g of FeCl 3 Dissolve in 4-6 mL of deionized water, add dropwise to the dopamine mixture through a dropping funnel, stir while adding dropwise, the stirring rate is 800-1000 r / min, add 0.8-1.6 g of triphenylsulfonium perfluorobutyl after the addition is completed, stir at room temperature for 30-60 min to obtain a UV dopamine adhesive.

6. A method for preparing a low volatile organic compound (VOCs) release, UV peelable sticker according to claim 1, Features: The specific process of step 5 is as follows: Take 1-2g of dopamine monomer and dissolve it in 10-15mL of N,N-dimethylformamide solvent, then add 1-2g of diethylene glycol ethyl ether acrylate, 0.1-0.3g of ethylene glycol dimethacrylate, and then add 10-20mg of catalyst, heat to 65-80℃ under nitrogen conditions for reaction for 30-45min, and cool to room temperature after the reaction to obtain oligomer dopamine.

7. A method for preparing a low volatile organic compound (VOCs) release, UV peelable sticker according to any one of claims 3 and 6, Features: The catalysts in step 2 and step 5 are both azobisisobutyronitrile.

8. A method for preparing a low volatile organic compound (VOCs) release, UV peelable sticker according to claim 1, Features: The specific process of step 6 is as follows: Take 5cmx10cm label paper, apply oligomer dopamine on the surface of the label paper by screen printing, with a coating thickness of 10-20um, irradiate the coated label with ultraviolet light for 10-20s, bake in an oven at 45°C for 12-18h, and print a layer of UV dopamine adhesive on the side of the sticker coated with oligomer dopamine by screen printing, with a coating thickness of 30-50um, to obtain a sticker with low VOCs release and UV peeling.