Drying-free water-based hot-melt corrugated paper adhesive and preparation method thereof
By using starch esterification and plasticization treatment in corrugated paper adhesives, hot melt adhesives are formed, which solves the instability and drying problems of corrugated paper adhesives, and achieves high-speed production and stable bonding strength, which is suitable for high-speed Production and recycling.
Patent Information
- Application Number
- CN202411214200.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-31
- Publication Date
- 2024-11-12
AI Technical Summary
The existing corrugated adhesives are unstable, resulting in unstable viscosity during high-speed production, poor initial adhesion effect, and uneven drying, which is prone to warping, softening or brittle cardboard, affecting production efficiency and quality.
Using dry-free water-based hot melt corrugated paper adhesive, the adhesive is solid particles, and is treated with starch esterification and composite plasticization, and is equipped with ethylene-vinyl acetate copolymer, tackifier additive and low melting point oxidative poly Ethylene wax forms a hot melt adhesive that can quickly melt into a slurry at room temperature, and is used for high-speed production without drying.
The stability and bonding strength of the adhesive are improved, the production process control is simplified, and the damage to the cardboard is avoided by drying is suitable for high-speed production, and is prone to disintegration during recycling, without affecting the cardboard treatment.
Smart Images

Figure CN118931426A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of functional adhesives, relates to corrugated paper adhesive technology, and specifically relates to a drying-free water-based hot-melt corrugated paper adhesive and a preparation method thereof. Background Art
[0002] Corrugated cardboard is made of surface paper and core paper that is processed by corrugating rollers to form a corrugated shape. Corrugated cardboard has the characteristics of light weight, low cost, and anti-punching, so it has become the preferred material for packaging boxes. According to different needs, corrugated paper has been formed into three-layer, five-layer, seven-layer, eleven-layer and other corrugated cardboards of different thicknesses.
[0003] Due to the large demand for corrugated paper, the production of corrugated paper requires high-speed bonding operation. The speed of general high-speed corrugated cardboard production lines exceeds 200m / min, which puts extremely high demands on high-speed bonding.
[0004] At present, the adhesive of corrugated paper is mainly a slurry adhesive obtained by gelatinizing starch, sodium hydroxide, borax, etc. in water. When using, the adhesive is applied to the flute and laminated with the surface paper. The adhesive quickly soaks the flute and the surface paper, and completes the bonding under sufficient heat and humidity conditions. The water evaporates under high temperature, and finally achieves complete bonding and curing. Therefore, the bonding of high-speed line corrugated paper requires the adhesive to dry quickly, have high solid content, low viscosity, and good initial adhesion.
[0005] However, the existing corrugated cardboard adhesives are unstable, which directly affects the high-speed production efficiency and quality of corrugated paper. It is mainly reflected in: 1. Unstable viscosity. During the use of the adhesive, the viscosity of the adhesive is unstable due to the influence of the placement time, environmental humidity, degree of gelatinization, changes in the degree of cross-linking, etc. If the ambient temperature is high, the adhesive will automatically oxidize and the viscosity will decrease, which not only affects the initial bonding effect, but also during high-speed bonding, the low viscosity is prone to adhesive throw-off, which will cause the cardboard to warp or soften, making it difficult to dry; if the viscosity is too high, the bonding infiltration will deteriorate, and the cardboard will become brittle after drying; 2. At present, the corrugated paper adhesive needs to be used up within 2-3 hours after preparation. If it is placed for a long time, it will cause excessive gelatinization, hydrolysis, oxidation, mesh blocking, etc. The oxidation depth is difficult to control, and the quality of the adhesive cannot be controlled, affecting the adhesive. Viscosity, coating amount changes, bonding strength changes, etc.; 3. Changes in the moisture content of corrugated paper will also significantly affect the curing time of the adhesive. In order to control the moisture content of the base paper at 9%-12% during corrugation forming, the moisture content of the base paper must be adjusted using a preheating roller and a spray device. The dynamic controllability of its operation is poor, resulting in poor bonding stability; 4. When corrugated paper is produced at high speed, the dryer cannot fully dry the adhesive due to the excessive speed, which can easily lead to problems such as cardboard debonding and false adhesion. Although rapid drying is achieved by increasing the drying temperature (the drying temperature has been increased to 180°C), high-temperature drying causes the cardboard to lose moisture, become dry, and become brittle.
[0006] Especially when preparing corrugated paper on a high-speed line, the adhesive is required to have a low viscosity. The viscosity measured by the 3# cup is controlled at around 20 seconds. Obviously, the low viscosity meets the rapid coating requirements of the high-speed line, but leads to difficulties in initial adhesion and the inevitable problem of debonding.
[0007] In general, the adhesive used to prepare corrugated paper is a water-based slurry, and its bonding relies on the penetration of the paper surface. Its penetration bonding determines that its process controllability and stability are poor. The phenomena of bubbling, degumming, and false adhesion of corrugated paperboard on the corrugated paperboard production line are mainly caused by the instability of the adhesive. Due to the instability of the adhesive, the corrugated paperboard production line produces a large amount of waste and defective products, which seriously hinders cost reduction and efficiency improvement. The moisture content of the base paper, the viscosity of the adhesive, the initial viscosity, drying and curing, and the speed matching of the vehicle affect the stable production of the corrugated paper high-speed line. Summary of the invention
[0008] In view of the technical problems existing in the current preparation of corrugated paper using starch slurry as an adhesive, the present invention proposes a drying-free water-based hot-melt corrugated paper adhesive, which is not a slurry of a water system, but an adhesive with hot-melt bonding properties. It is solid particles at room temperature and quickly melts into a slurry when heated when used. There are no special requirements for the temperature and moisture of the base paper during bonding, and it can be used for high-speed production of corrugated paper without drying. Furthermore, a preparation method of the adhesive is provided.
[0009] In order to achieve the above-mentioned technical effects, the technical solution adopted by the present invention is:
[0010] First, a method for preparing a drying-free water-based hot-melt corrugated paper adhesive is provided. The specific preparation method is as follows:
[0011] S1. Raw material preparation:
[0012] Weigh the raw materials according to weight: 70-75 parts of native starch, 5-8 parts of composite plasticizer, 3-5 parts of polyvinyl alcohol, 3-5 parts of ethylene-vinyl acetate copolymer, 2-3 parts of viscosity-increasing agent, 0.5-1 parts of low-melting-point oxidized polyethylene wax, 0.2-0.5 parts of maleic anhydride, 0.1-0.3 parts of flake caustic soda, 0.05-0.1 parts of cross-linking agent, 0.05-0.1 parts of antioxidant, and 30-40 parts of purified water;
[0013] S2. Add polyvinyl alcohol and caustic soda to pure water and soak until the polyvinyl alcohol is completely dissolved to obtain a polyvinyl alcohol glue for later use;
[0014] S3. Add the original starch, composite plasticizer, and maleic anhydride into the mixer, close the lid, stir in a closed state for 10-15 minutes, add the polyvinyl alcohol glue prepared in step S2, heat and stir under closed conditions, control the temperature to 80°C, and stir until the original starch is gelatinized and becomes agglomerate; add ethylene-vinyl acetate copolymer, viscosity-enhancing agent, low-melting-point oxidized polyethylene wax, cross-linking agent, and antioxidant, control the temperature to 100°C, open the vent hole of the lid, stir and exhaust under non-closed conditions until the water content is 8-10%, and discharge;
[0015] S4. The material obtained in step S3 is naturally cooled and then crushed to obtain a granular adhesive, that is, a water-based hot-melt corrugated paper adhesive that does not require drying.
[0016] The native starch is selected from at least one of corn starch and tapioca starch.
[0017] The composite plasticizer is prepared by mixing ethylene glycol or / and glycerol with dimethyl sulfoxide in a mass ratio of 3:1. The composite plasticizer deeply reacts with starch hydroxyl groups to promote good thermoplasticity and adhesion of starch.
[0018] The polyvinyl alcohol is a water-soluble polyvinyl alcohol with an alcoholysis degree of 78-92%, and the particularly preferred grades are 17-88, 17-92, and 24-88.
[0019] The ethylene-vinyl acetate copolymer is selected from ethylene-vinyl acetate copolymers having a melt index of ≥1000g / 10min and a VA content of ≥40%.
[0020] The tackifying aid is selected from at least one of rosin resin, maleic rosin, terpene resin, and E-20 epoxy resin, and is used to increase the initial tackiness of corrugated paper during high-speed line production.
[0021] The low melting point oxidized polyethylene wax is selected to have a melting point lower than 50° C. The low melting point oxidized polyethylene wax not only promotes the adhesion of corrugated paper, but also promotes the hot melt flow of the adhesive and increases the uniformity of the adhesive on the coating roller.
[0022] The cross-linking agent is selected from at least one of borax, dicumyl peroxide, benzoyl peroxide and di-tert-butyl peroxide.
[0023] The antioxidant is selected from at least one of BHT (2,6-di-tert-butyl-4-methylphenol), 264 (2,6-di-tert-butyl-4-methylphenol), 1010 [β-(3,5-di-tert-butyl-4-hydroxyphenyl) pentaerythritol ester], 168 [tris(2.4-di-tert-butylphenyl) phosphite], and TNPP [tris(nonylphenyl) phosphite]; and it is particularly preferred that 1010 [β-(3,5-di-tert-butyl-4-hydroxyphenyl) pentaerythritol ester] and 168 [tris(2.4-di-tert-butylphenyl) phosphite] are used in combination.
[0024] Preferably, in step S2, polyvinyl alcohol and caustic soda are added to pure water and soaked for more than 12 hours until the polyvinyl alcohol is completely dissolved. The basis for judgment is that the glue is fine and there are no undissolved particles. Further, in order to speed up the dissolution of polyvinyl alcohol, low-speed stirring can be performed.
[0025] Furthermore, the present invention provides a drying-free water-based hot-melt corrugated paper adhesive prepared by the above-mentioned preparation method. In view of the fact that traditional corrugated paper adhesives use starch slurry, bonding is difficult to control, and the adhesive viscosity, base paper moisture content, and temperature are required to be high, and high-speed line production and drying are difficult to control and other technical problems. The drying-free water-based hot-melt corrugated paper adhesive proposed by the present invention is obtained by esterifying the original starch, compounding and plasticizing, and assisting with hot-melt additives. The adhesive is in a solid granular state. When used, it is heated and melted into a high-fluidity hot melt adhesive. It has good hot melt and adhesion properties, can quickly adhere to the flute peaks, and achieve high-speed bonding of corrugated paper. It does not require heating of the base paper, does not require controlling the moisture content of the base paper, and does not require drying.
[0026] The main material of the drying-free water-based hot-melt corrugated paper adhesive of the present invention is still starch, and the water resistance of the bonded corrugated paper is better than that of the starch slurry adhesive. When the corrugated paper is recycled and reused, the adhesive is easily disintegrated and dissolved in water, and does not affect the recycling of the paperboard.
[0027] Due to the huge difference in the use methods between the drying-free water-based hot-melt corrugated paper adhesive of the present invention and the traditional starch slurry adhesive, the present invention recommends the typical use method as follows:
[0028] (1) adding the drying-free water-based hot-melt corrugated paper adhesive into a screw extruder, hot-melt extruding at 80-100° C., and casting the adhesive onto a coating roller through a T-die to be evenly distributed;
[0029] (2) According to the thickness of the corrugated paper, the distance between the coating rollers is adjusted. When the corrugated core paper passes through the coating roller, the adhesive of the coating roller is coated on the flute peaks, and the surface paper is bonded while hot. After being flattened and pressed by the leveling roller, the preparation of the corrugated paper is completed.
[0030] Obviously, the drying-free water-based hot-melt corrugated paper adhesive of the present invention greatly simplifies the control of the preparation process of corrugated paperboard. The continuous feeding of hot-melt extrusion by the screw extruder ensures the stability of the adhesive, and the hot-melt adhesive is attached to the interface bonding, does not require penetration, can quickly adhere to the flute peak, and realizes high-speed bonding of corrugated paper, does not require heating of the base paper, does not require control of the base paper moisture, and does not require drying.
[0031] Compared with the prior art, the present invention has the following outstanding features and significant advantages:
[0032] 1. The present invention proposes a water-based hot-melt corrugated paper adhesive that does not require drying. Starch is esterified and plasticized to become a hot-melt adhesive. Through the coordinated auxiliary ethylene-vinyl acetate copolymer, a tackifier, and a low-melting-point oxidized polyethylene wax, the obtained adhesive is easy to hot-melt flow, easy to evenly disperse and coat, and easy to bond.
[0033] 2. The drying-free water-based hot-melt corrugated paper adhesive proposed in the present invention greatly simplifies the control of the preparation process of corrugated paperboard. It continuously feeds the material by hot-melt extrusion through a screw extruder, thereby ensuring the stability of the adhesive. Moreover, the hot-melt adhesive is only for interface bonding, and does not require penetration. It can quickly adhere to the flute peaks, thereby achieving high-speed bonding of corrugated paper. It does not require heating of the base paper, controlling the moisture content of the base paper, or drying.
[0034] 3. The drying-free water-based hot-melt corrugated paper adhesive proposed by the present invention still has starch as the main material, and the water resistance of the bonded corrugated paper is better than that of the starch slurry adhesive. When the corrugated paper is recycled and reused, the adhesive is easily disintegrated and dissolved in water, and does not affect the recycling of the paperboard.
[0035] 4. The preparation process of the present invention is easy to control and can be continuously mass-produced. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] In order to further clarify the drying-free water-based hot-melt corrugated paper adhesive of the present invention, the present invention is further described below in conjunction with the accompanying drawings:
[0037] Figure 1 It is a photo of the water-based hot-melt corrugated paper adhesive of the present invention that does not require drying.
[0038] Figure 2 This is a photograph of the corrugated paper bonded with the adhesive in Example 1 being peeled off.
[0039] Figure 3 This is a photo of the corrugated paper peeled off after being bonded with the adhesive in Comparative Example 1. DETAILED DESCRIPTION
[0040] The following examples are intended to further describe the implementation process of the technical content of the present invention, but are not intended to limit the scope of protection of the claims of the present invention. If no specific conditions are specified in the examples, conventional process conditions are used.
[0041] Example 1
[0042] S1. Raw material preparation:
[0043] Weigh the raw materials according to weight: 70 parts of corn starch, 6 parts of composite plasticizer (glycerol and dimethyl sulfoxide are compounded in a mass ratio of 3:1), 5 parts of 17-88 polyvinyl alcohol, 3 parts of ethylene-vinyl acetate copolymer (melt index ≥1000g / 10min, VA content ≥40%), 2 parts of E-20 epoxy resin, 0.8 parts of low-melting point oxidized polyethylene wax, 0.5 parts of maleic anhydride, 0.1 parts of flake caustic soda, 0.05 parts of cross-linking agent borax, 0.05 parts of β-(3,5-di-tert-butyl-4-hydroxyphenyl) pentaerythritol ester antioxidant, 0.05 parts of tris(2.4-di-tert-butylphenyl) phosphite antioxidant, and 35 parts of purified water;
[0044] S2. Add polyvinyl alcohol and alkali flakes to pure water and soak until the polyvinyl alcohol is completely dissolved to obtain a fine polyvinyl alcohol glue for later use;
[0045] S3. Add corn starch, composite plasticizer, and maleic anhydride to the mixer, close the lid, stir for 15 minutes, add the polyvinyl alcohol glue prepared in step S2, heat and stir under closed conditions, control the temperature to 80°C, and stir for 25 minutes until the corn starch gelatinizes and becomes a light yellow translucent mass; add ethylene-vinyl acetate copolymer, E-20 epoxy resin, low melting point oxidized polyethylene wax, crosslinking agent, and antioxidant, control the temperature to 100°C, open the lid vent, stir and exhaust under non-closed conditions to 8-10% water content, and discharge;
[0046] S4. The material obtained in step S3 is naturally cooled and then crushed to obtain a light yellow translucent granular adhesive (such as attached Figure 1 ), which is a water-based hot-melt corrugated paper adhesive that does not require drying.
[0047] The melt index of the adhesive tested at 125°C and 0.325kg pressure is 926g / 10min; the melt index of the adhesive tested at 100°C and 0.325kg pressure is 834g / 10min. The obtained adhesive has excellent hot melt fluidity and is suitable for evenly adhering to corrugated paper after hot melt coating. The surface paper and the core paper are firmly bonded and not easy to peel off. Figure 2 .
[0048] Example 2
[0049] S1. Raw material preparation:
[0050] Weigh the raw materials according to weight: 75 parts of corn starch, 8 parts of composite plasticizer (ethylene glycol and dimethyl sulfoxide are compounded in a mass ratio of 3:1), 4 parts of 17-88 polyvinyl alcohol, 5 parts of ethylene-vinyl acetate copolymer (melt index ≥1000g / 10min, VA content ≥40%), 3 parts of maleic rosin, 0.8 parts of low-melting-point oxidized polyethylene wax, 0.3 parts of maleic anhydride, 0.2 parts of flake caustic soda, 0.05 parts of cross-linking agent borax, 0.05 parts of β-(3,5-di-tert-butyl-4-hydroxyphenyl) pentaerythritol ester antioxidant, 0.05 parts of tris(2.4-di-tert-butylphenyl) phosphite antioxidant, and 40 parts of purified water;
[0051] S2. Add polyvinyl alcohol and alkali flakes to pure water and soak until the polyvinyl alcohol is completely dissolved to obtain a fine polyvinyl alcohol glue for later use;
[0052] S3. Add corn starch, composite plasticizer, and maleic anhydride to the mixer, close the lid, stir for 15 minutes, add the polyvinyl alcohol glue prepared in step S2, heat and stir under closed conditions, control the temperature to 80°C, stir for 25 minutes until the corn starch gelatinizes and becomes a light yellow translucent mass; add ethylene-vinyl acetate copolymer, maleic rosin, low melting point oxidized polyethylene wax, crosslinking agent, and antioxidant, control the temperature to 100°C, open the lid vent, stir and exhaust under non-closed conditions to 8-10% water content, and discharge;
[0053] S4. The material obtained in step S3 is naturally cooled and then crushed to obtain a light yellow translucent granular adhesive, that is, a water-based hot-melt corrugated paper adhesive that does not require drying.
[0054] The melt index of the adhesive tested at 125°C and 0.325kg pressure is 976g / 10min; the melt index of the adhesive tested at 100°C and 0.325kg pressure is 858g / 10min; the obtained adhesive has excellent hot melt fluidity and is suitable for adhering to corrugated paper after hot melt coating roller.
[0055] Example 3
[0056] S1. Raw material preparation:
[0057] Weigh the raw materials according to weight: 70 parts of cassava corn starch, 6 parts of composite plasticizer (glycerol and dimethyl sulfoxide are compounded in a mass ratio of 3:1), 5 parts of 24-88 polyvinyl alcohol, 5 parts of ethylene-vinyl acetate copolymer (melt index ≥1000g / 10min, VA content ≥40%), 3 parts of terpene resin, 1 part of low-melting point oxidized polyethylene wax, 0.4 parts of maleic anhydride, 0.3 parts of caustic soda, 0.05 parts of cross-linking agent diisopropyl peroxide, 0.05 parts of β-(3,5-di-tert-butyl-4-hydroxyphenyl) pentaerythritol ester antioxidant, 0.05 parts of tris(2.4-di-tert-butylphenyl) phosphite antioxidant, and 30 parts of purified water;
[0058] S2. Add polyvinyl alcohol and alkali flakes to pure water and soak until the polyvinyl alcohol is completely dissolved to obtain a fine polyvinyl alcohol glue for later use;
[0059] S3. Add cassava starch, composite plasticizer, and maleic anhydride to the mixer, close the lid, stir in a closed state for 10 minutes, add the polyvinyl alcohol glue prepared in step S2, heat and stir under closed conditions, control the temperature to 80°C, and stir for 30 minutes until the cassava starch is gelatinized and becomes a light red translucent mass; add ethylene-vinyl acetate copolymer, terpene resin, low melting point oxidized polyethylene wax, crosslinking agent, and antioxidant, control the temperature to 100°C, open the vent hole of the lid, stir and exhaust under non-closed conditions to 8-10% water content, and discharge;
[0060] S4. The material obtained in step S3 is naturally cooled and then crushed to obtain a light red translucent granular adhesive, that is, a water-based hot-melt corrugated paper adhesive that does not require drying.
[0061] The melt index of the adhesive tested at 125°C and 0.325kg pressure is 1008g / 10min; the melt index of the adhesive tested at 100°C and 0.325kg pressure is 951g / 10min; the obtained adhesive has excellent hot melt fluidity and is suitable for adhering to corrugated paper after hot melt coating roller.
[0062] Comparative Example 1
[0063] The preparation method is consistent with that in Example 1, except that no composite plasticizer is used in the raw materials.
[0064] The prepared adhesive has a melt index of 692g / 10min at 125°C and 0.325kg pressure; the melt index of 455g / 10min at 100°C and 0.325kg pressure. The plasticization effect of the obtained adhesive is poor, the hot melt fluidity is low, unplasticized starch particles exist when bonding corrugated paper, and coating is difficult, the bonding strength is greatly reduced, and the surface paper and the core paper are easy to be unbonded and peeled off. Figure 3 .
[0065] Comparative Example 2
[0066] The preparation method is consistent with that of Example 1, except that maleic anhydride is not used in the raw materials.
[0067] The melt index of the prepared adhesive tested at 125°C and 0.325kg pressure was 711g / 10min; the melt index of the adhesive tested at 100°C and 0.325kg pressure was 483g / 10min; the obtained adhesive had poor thermoplasticity and was difficult to apply because it was not esterified.
[0068] Comparative Example 3
[0069] The preparation method is consistent with that of Example 1, except that E-20 epoxy resin and low melting point oxidized polyethylene wax are not used in the raw materials.
[0070] The melt index of the prepared adhesive tested at 125°C and 0.325kg pressure was 486g / 10min; the melt index of the adhesive tested at 100°C and 0.325kg pressure was 277g / 10min; the fluidity of the obtained adhesive deteriorated, the uniformity of roller coating decreased, resulting in reduced bonding strength.
[0071] Comparative Example 4
[0072] The preparation method is consistent with that in Example 1, except that ethylene-vinyl acetate copolymer is not used in the raw materials.
[0073] The melt index of the prepared adhesive tested at 125°C and 0.325kg pressure was 655g / 10min; the melt index of the adhesive tested at 100°C and 0.325kg pressure was 426g / 10min; the fluidity of the obtained adhesive deteriorated and the bonding strength decreased.
[0074] The adhesives obtained from Examples 1-3 and Comparative Examples 1-4 were used for comparative testing of the adhesive properties of corrugated cardboard, and the adhesive strength test was performed with reference to GB / T6548 "Determination of Adhesive Strength of Corrugated Cardboard". The corrugation of the sample to be tested was facing upward, and a metal test needle was used to align the midpoint of the corrugated corrugation peak, and pressure was applied at a speed of 12.5 mm / min. The adhesive strength was calculated according to the formula A=F / L, where A is the adhesive strength, in N / m; F is the maximum force when the sample is separated, in N; and L is the sample length, in m. The test data is shown in Table 1:
[0075] Table 1:
[0076]
[0077] Performance tests have shown that the drying-free water-based hot-melt corrugated paper adhesive of the present invention is prepared by esterifying and plasticizing starch, and by coordinating ethylene-vinyl acetate copolymer, a tackifying aid, and a low-melting-point oxidized polyethylene wax to obtain an adhesive with excellent hot-melt flowability, suitable for uniformly adhering to corrugated paper after a hot-melt coating roller, and having high bonding strength between the face paper and the core paper, and is particularly suitable for the production of high-bonding-strength, high-speed corrugated paper.
[0078] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing a water-based hot-melt corrugated paper adhesive that does not require drying. The specific preparation method is as follows: S1. Raw material preparation: Weigh the raw materials according to weight: 70-75 parts of native starch, 5-8 parts of composite plasticizer, 3-5 parts of polyvinyl alcohol, 3-5 parts of ethylene-vinyl acetate copolymer, 2-3 parts of viscosity-increasing agent, 0.5-1 parts of low-melting-point oxidized polyethylene wax, 0.2-0.5 parts of maleic anhydride, 0.1-0.3 parts of flake caustic soda, 0.05-0.1 parts of cross-linking agent, 0.05-0.1 parts of antioxidant, and 30-40 parts of purified water; S2. Add polyvinyl alcohol and caustic soda to pure water and soak until the polyvinyl alcohol is completely dissolved to obtain a polyvinyl alcohol glue for later use; S3. Add the original starch, composite plasticizer, and maleic anhydride to the mixer, close the lid, stir in a closed state for 10-15 minutes, add the polyvinyl alcohol glue prepared in step S2, heat and stir under closed conditions, control the temperature to 80°C, and stir until the original starch is gelatinized and becomes agglomerate; add ethylene-vinyl acetate copolymer, viscosity-enhancing agent, low-melting-point oxidized polyethylene wax, cross-linking agent, and antioxidant, control the temperature to 100°C, open the vent hole of the lid, stir and exhaust under non-closed conditions to 8-10% water content, and discharge; S4. The material obtained in step S3 is naturally cooled and then crushed to obtain a granular adhesive, that is, a water-based hot-melt corrugated paper adhesive that does not require drying.
2. The method for preparing a drying-free aqueous hot-melt corrugated paper adhesive according to claim 1, characterized in that: The native starch is selected from at least one of corn starch and tapioca starch.
3. The method for preparing a drying-free aqueous hot-melt corrugated paper adhesive according to claim 1, characterized in that: The composite plasticizer is prepared by mixing ethylene glycol or / and glycerol with dimethyl sulfoxide in a mass ratio of 3:
1.
4. The method for preparing a drying-free aqueous hot-melt corrugated paper adhesive according to claim 1, characterized in that: The polyvinyl alcohol is a water-soluble polyvinyl alcohol with an alcoholysis degree of 78-92%.
5. The method for preparing a drying-free water-based hot-melt corrugated paper adhesive according to claim 1, characterized in that: The ethylene-vinyl acetate copolymer is selected from ethylene-vinyl acetate copolymers having a melt index of ≥1000g / 10min and a VA content of ≥40%.
6. The method for preparing a drying-free water-based hot-melt corrugated paper adhesive according to claim 1, characterized in that: The tackifying aid is selected from at least one of rosin resin, maleic rosin, terpene resin, and E-20 epoxy resin.
7. The method for preparing a drying-free water-based hot-melt corrugated paper adhesive according to claim 1, characterized in that: The low melting point oxidized polyethylene wax is selected from low melting point oxidized polyethylene wax having a melting point lower than 50°C.
8. The method for preparing a drying-free water-based hot-melt corrugated paper adhesive according to claim 1, characterized in that: The cross-linking agent is selected from at least one of borax, dicumyl peroxide, benzoyl peroxide and di-tert-butyl peroxide.
9. The method for preparing a drying-free water-based hot-melt corrugated paper adhesive according to claim 1, characterized in that: The antioxidant is selected from at least one of BHT, 264, 1010, TNPP, and 168.
10. The drying-free water-based hot-melt corrugated paper adhesive obtained by the preparation method according to any one of claims 1 to 9.