Acrylate electromagnetic shielding adhesive tape and preparation method thereof
By using high acid acrylate adhesives and modified metal particles in electromagnetic shielding tape, the bonding strength and conductivity problems of electromagnetic shielding tape in the prior art under lightweight and high frequency environments are solved, and efficient Electromagnetic shielding performance and shelf life are extended.
Patent Information
- Application Number
- CN202411027397.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-12
AI Technical Summary
Existing electromagnetic shielding tapes are difficult to maintain high bonding strength and conductivity in the pursuit of lightweight and high frequency electromagnetic wave environments, and the reduction in material thickness will affect the shielding performance.
High acid acrylate adhesives and modified metal particles are used to coat polyaniline on the surface, and the conductive and adhesive strength of the tape is improved through specific preparation methods, including the use of high acid poly at 50% solids content Acrylate adhesives and modified metal particles are combined with silane coupling agent pretreatment and oxidant coating to form an efficient electromagnetic shielding tape.
It achieves high bonding strength and conductivity under low thickness, extends the shelf life of the tape, and improves electromagnetic shielding performance, and is suitable for oily and water-based acrylate systems.
Smart Images

Figure CN118931434A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electromagnetic shielding tapes, and in particular to an acrylic electromagnetic shielding tape and a preparation method thereof. Background Art
[0002] With the promotion of 5G technology and the continuous rise of superconducting technology, base station equipment and signal transmission technologies must also be continuously upgraded, which will inevitably lead to the intensification of electromagnetic interference, and the need to use convenient and efficient electromagnetic shielding products. In addition, as the performance requirements of electronic products continue to increase, such as faster computing speeds, higher resolutions, more auxiliary functions, and even higher artificial intelligence, this requires that the various components of electronic products need to be able to operate stably and efficiently under higher and wider frequency electromagnetic waves. It is also necessary to protect each component with electromagnetic shielding to prevent abnormal signal transmission from causing abnormal component function. On the other hand, electronic products are also constantly developing in the direction of lightweight, which requires various components to be assembled on smaller circuit boards. Traditional shielding methods such as metal shells will no longer be applicable, and corresponding requirements for lightweight shielding products have also been put forward.
[0003] At present, electromagnetic shielding tapes are often used in electronic products to protect components with both bonding and electromagnetic shielding functions, such as the "Electromagnetic shielding tape and method for preparing electromagnetic shielding tape" disclosed in the Chinese invention patent application with patent number CN201710243555.2 (publication number CN106987218A), and the "Method for preparing a carbon nanosphere-filled dual-cured conductive tape and its application in electromagnetic shielding tape" disclosed in the Chinese invention patent application with patent number CN201910496662.5 (publication number CN110408342A).
[0004] However, as the space reserved for electromagnetic shielding materials in electronic products continues to shrink with the development trend of lightweighting, in order to ensure the effect of electromagnetic shielding, the contact area between the material and the electromagnetic product cannot be changed, and space can only be saved by reducing the thickness of the material. If the thickness of the substrate layer is reduced, the electromagnetic shielding performance will be greatly reduced, and if the thickness of the adhesive layer is reduced, the bonding performance will be affected. Therefore, how to ensure the bonding performance of the conductive tape while adding high particles and low thickness has become a technical problem for existing electromagnetic shielding tapes. Summary of the invention
[0005] The first technical problem to be solved by the present invention is to provide an acrylic electromagnetic shielding tape with high bonding strength and good electrical conductivity in view of the current status of the prior art.
[0006] The second technical problem to be solved by the present invention is to provide a method for preparing the above-mentioned acrylic electromagnetic shielding tape in view of the current status of the prior art.
[0007] The technical solution adopted by the present invention to solve the above-mentioned first technical problem is: an acrylic electromagnetic shielding tape, characterized in that it includes an adhesive layer, and the adhesive layer includes, by weight,
[0008]
[0009] When the solid content is 50%, the acid value of the high acid value polyacrylate adhesive ranges from 21.7 to 66.7 mg KOH / g;
[0010] The modified metal particles are metal particles whose surfaces are coated with polyaniline.
[0011] Preferably, the modified metal particles include, by mass:
[0012]
[0013] Preferably, the metal particles are at least one of iron powder, nickel powder and copper powder, and the size is preferably between 3 and 5 um;
[0014] The oxidant is at least one of hydrogen peroxide, potassium dichromate, ammonium persulfate, potassium iodate, and potassium permanganate, preferably ammonium persulfate. The solvent is at least one of hydrochloric acid, an aqueous phosphoric acid solution, an aqueous dodecylbenzenesulfonic acid solution, and an aqueous dioctyl succinate sulfonic acid solution, preferably hydrochloric acid, and the concentration is 1 mol / L.
[0015] Because metal ions are highly active, the metal particles are pretreated with a silane coupling agent KH-550. The pretreatment method is as follows: iron powder or nickel powder and the silane coupling agent are added to a 90% ethanol solution in a ratio of 3:1 to 5:1, and an acid solution is added to adjust the pH to 4. After stirring for 8 to 12 hours to make it fully uniform, the mixture is filtered, washed with a 90% ethanol solution for 3 to 5 times, and dried for later use.
[0016] Preferably, the method for preparing the modified metal particles comprises the following steps:
[0017] (1) Dividing deionized water into two parts, adding metal particles into the first part of deionized water according to a certain proportion, and performing ultrasonic homogenization to form a metal particle dispersion;
[0018] (2) adding the metal particle dispersion, aniline, and solvent into a reaction vessel in sequence, and stirring for 4 to 6 hours under an ice bath to form a mixed solution;
[0019] (3) adding an oxidant to the second portion of deionized water and stirring to form an oxidant solution;
[0020] (4) adding the oxidant solution to the mixed solution, stirring for 2 h to 4 h in an ice bath, then heating to room temperature, washing with deionized water for 3 to 5 times, and centrifuging at 5000 rpm for 0.5 to 1 h after the washing solution becomes colorless, to finally obtain modified metal particles coated with polyaniline on the surface.
[0021] Preferably, the high acid value polyacrylate adhesive comprises, by weight:
[0022]
[0023] Preferably, the initiator is azobisisobutyronitrile (AIBN), and the solvent is ethyl acetate.
[0024] Preferably, the method for preparing the high acid value polyacrylate adhesive comprises the following steps:
[0025] (1) Dividing the solvent into two parts, adding the above-mentioned isooctyl acrylate, 2-hydroxyethyl acrylate, butyl acrylate, acrylic acid, methyl methacrylate and the first part of the solvent into a reaction container in proportion, and stirring at a constant temperature of 80 to 90° C. for 1 to 3 hours in a N2 atmosphere to form a mixed solution;
[0026] (2) adding the initiator AIBN to the second part of the solvent to prepare an initiator solution according to the above-mentioned number of portions;
[0027] (3) adding half of the initiator solution to the mixed solution and reacting at 80-90° C. for 1-2 h;
[0028] (4) adding the remaining initiator solution and reacting at 80-90° C. for another 4-6 hours;
[0029] (5) cooling to 30-40° C., filtering while hot, and obtaining the high acid value polyacrylate adhesive.
[0030] Preferably, the resin is rosin resin, which is dissolved in ethyl acetate to form a resin solution; the curing agent is at least one of toluene diisocyanate (TDI), hexamethylene diisocyanate (HDI), and 4,4'-dicyclohexylmethane diisocyanate (HMDI); and the antioxidant is benzotriazole, which is dissolved in ethyl acetate to form an antioxidant solution.
[0031] The technical solution adopted by the present invention to solve the above second technical problem is: the adhesive tape further includes a substrate layer and a release layer, and the preparation method of the adhesive tape includes the following steps:
[0032] (1) adding a high acid value polyacrylate adhesive, a tackifying resin solution, an antioxidant solution, and modified metal particles into a reaction container in proportion and stirring them uniformly to form a mixed solution;
[0033] (2) adding the curing agent to the mixed solution in proportion, stirring evenly to form a mixture;
[0034] (3) applying the mixture on the release layer to a coating thickness of 15±1 μm, and then placing it in a drying oven to remove the solvent to obtain an adhesive / release layer;
[0035] (4) After the dried adhesive / release layer is taken out, the adhesive is pasted on the substrate layer; the substrate layer can be a metal foil with a thickness of 30±2 μm
[0036] (5) Then, the mixture is placed in a drying oven at 40° C. and aged for 2 to 3 days to obtain the acrylic electromagnetic shielding tape.
[0037] Compared with the prior art, the advantages of the present invention are as follows: First, the present invention coats the surface of metal particles with polyaniline, which, as a conductive polymer material, will not significantly reduce its conductivity, and will not dissolve in ethyl acetate and water, and has a certain heat resistance, and can be applied to oily acrylates, water-based acrylates and hot-melt acrylates; at the same time, the present invention introduces polyaniline to coat the metal particles, especially the coating of the metal particles, which can effectively prevent the particles from being oxidized or even rusted, thereby effectively extending the shelf life of the tape;
[0038] Second: Commonly used acrylic adhesives have a small amount of acidity or no acidity. The polyacrylate adhesive designed and prepared by the present invention has a higher acid value and can react with polyaniline, which can not only form ionic bonds and increase the interaction between metal particles and adhesives, thereby effectively improving the dispersion of particles, and ultimately improving the bonding strength of the tape or further increasing the amount of particles added, but also can make more nitrogen atoms on polyaniline protonated to form more charged excited state polarons, thereby improving conductivity to a certain extent. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 Schematic diagram of the resistance testing device. DETAILED DESCRIPTION
[0040] The present invention is further described in detail below with reference to the accompanying drawings.
[0041] The acrylic electromagnetic shielding tape of the present invention comprises an adhesive layer, a substrate layer and a release layer.
[0042] The adhesive layer is calculated by weight, including
[0043]
[0044] At a solid content of 50%, the acid value of high acid polyacrylate adhesives ranges from 21.7 to 66.7 mg KOH / g;
[0045] High acid value polyacrylate adhesives, calculated by weight, include:
[0046]
[0047]
[0048] The initiator is azobisisobutylonitrile (AIBN), and the solvent is ethyl acetate.
[0049] The preparation method of a high acid value polyacrylate adhesive comprises the following steps:
[0050] (1) Dividing the solvent into two parts, adding the above-mentioned isooctyl acrylate, 2-hydroxyethyl acrylate, butyl acrylate, acrylic acid, methyl methacrylate and the first part of the solvent into a reaction container in proportion, and stirring at a constant temperature of 80 to 90° C. for 1 to 3 hours in a N2 atmosphere to form a mixed solution;
[0051] (2) adding the initiator AIBN to the second part of the solvent to prepare an initiator solution according to the above-mentioned number of portions; the mass fraction of the initiator in the solvent is 15%, and the subsequent storage time of the initiator solution is less than 2 hours;
[0052] (3) adding half of the initiator solution to the mixed solution and reacting at 80-90° C. for 1-2 h;
[0053] (4) adding the remaining initiator solution and reacting at 80-90° C. for another 4-6 hours;
[0054] (5) cooling to 30-40° C., filtering while hot, and obtaining the high acid value polyacrylate adhesive.
[0055] The modified metal particles are metal particles whose surfaces are coated with polyaniline. The modified metal particles, calculated by weight, include:
[0056] The preparation method of the modified metal ion comprises the following steps:
[0057] (1) Dividing deionized water into two parts, adding metal particles into the first part of deionized water according to a certain proportion, and performing ultrasonic homogenization to form a metal particle dispersion;
[0058] (2) adding the metal particle dispersion, aniline, and solvent into a reaction vessel in sequence, and stirring for 4 to 6 hours under an ice bath to form a mixed solution;
[0059] (3) adding an oxidant to the second portion of deionized water and stirring to form an oxidant solution;
[0060] (4) adding the oxidant solution to the mixed solution, stirring for 2 h to 4 h in an ice bath, then heating to room temperature, washing with deionized water for 3 to 5 times, and centrifuging at 5000 rpm for 0.5 to 1 h after the washing solution becomes colorless, to finally obtain modified metal particles coated with polyaniline on the surface.
[0061] The metal particles are pretreated using a silane coupling agent KH-550. The pretreatment method is as follows: iron powder or nickel powder and the silane coupling agent are added to a 90% ethanol solution at a ratio of 3:1 to 5:1, and an acid solution is added to adjust the pH to 4. After stirring for 8 to 12 hours to make it fully uniform, the mixture is filtered, washed with a 90% ethanol solution for 3 to 5 times, and dried for later use.
[0062] The resin used in the present invention is rosin resin, and the solvent is ethyl acetate. The tackifying resin is first dissolved in the solvent and then added into the adhesive, wherein the ratio of the tackifying resin to the solvent is 1:1.
[0063] The antioxidant used in the present invention is benzotriazole, and the selected solvent is ethyl acetate. The benzotriazole is dissolved in ethyl acetate and then added into the adhesive, wherein the ratio of benzotriazole to the solvent is 1:10.
[0064] The preparation method of the acrylic electromagnetic shielding tape comprises the following steps:
[0065] (1) adding a high acid value polyacrylate adhesive, a tackifying resin solution, an antioxidant solution, and modified metal particles into a reaction container in proportion and stirring them uniformly to form a mixed solution;
[0066] (2) adding the curing agent to the mixed solution in proportion, stirring evenly to form a mixture;
[0067] (3) applying the mixture onto the release layer and then placing it in a drying oven to remove the solvent to form an adhesive / release layer;
[0068] (4) After the dried adhesive / release layer is removed, the adhesive is adhered to the substrate layer;
[0069] (5) Then, the mixture is placed in a drying oven at 40° C. and aged for 2 to 3 days to obtain the acrylic electromagnetic shielding tape.
[0070] The aniline (C6H7N) used in the comparative example of the above embodiment was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd. (chemically pure), and the silane coupling agent KH-550 was purchased from Shin-Etsu Chemical Co., Ltd. of Japan.
[0071] As shown in the attached table, the present invention includes 8 embodiments and 6 comparative examples. The type and amount of the substance added in each embodiment, as well as the peel strength, resistance, and electromagnetic shielding effectiveness of the final adhesive tape are listed in the table.
[0072] The amount of each substance in the table without indicating the unit is weight percentage; the acid value in Table 1 is determined by titration, and the peel strength test standard is GB2792-2014; the resistance test method is as shown in the attached Figure 1 As shown in the figure, 1 is metal foil, 2 is test tape, and 3 is metal foil. Attach the test tape to the metal foil with the distance and size as shown in the attached figure. Figure 1 As shown, the AC two-point test value is the XY direction resistance, and the AB two-point test value is the Z direction resistance; the shielding effectiveness test standard is the flange coaxial device method in GJB 6190-2008. Comparative Examples II, III, and VI in the table cannot be prepared into finished tapes due to poor film-forming properties of the adhesive, so there are no corresponding performance results.
[0073] From the table, we can find that aniline can be successfully coated on the surface of metal particles to increase the dispersion ability of the particles, thereby increasing the filling amount of the particles, but excessive aniline will also reduce the conductivity of the particles. In addition, choosing an acrylic adhesive with a higher acid value can also effectively improve the dispersion and conductivity of the particles, but too high an acid value will reduce the peel strength.
[0074]
[0075]
[0076]
Claims
1. An acrylic electromagnetic shielding tape, characterized in that: Comprising an adhesive layer, the adhesive layer comprises, by weight, When the solid content is 50%, the acid value of the high acid value polyacrylate adhesive ranges from 21.7 to 66.7 mg KOH / g; The modified metal particles are metal particles whose surfaces are coated with polyaniline.
2. The acrylic electromagnetic shielding tape according to claim 1, characterized in that: The modified metal particles include, by weight, 3. The acrylic electromagnetic shielding tape according to claim 2, characterized in that: The metal particles are at least one of iron powder, nickel powder, and copper powder; the oxidant is at least one of hydrogen peroxide, potassium dichromate, ammonium persulfate, potassium iodate, and potassium permanganate; and the solvent is at least one of hydrochloric acid, phosphoric acid aqueous solution, dodecylbenzenesulfonic acid aqueous solution, and dioctyl succinate sulfonic acid aqueous solution.
4. The acrylic electromagnetic shielding tape according to claim 3, characterized in that: The metal particles are pretreated with silane coupling agent KH-550. The pretreatment method is: adding iron powder or nickel powder and silane coupling agent into ethanol solution, adding acid solution to adjust to acidity, stirring evenly, filtering, washing with ethanol solution, and drying for use.
5. The acrylic electromagnetic shielding tape according to claim 2, characterized in that: The preparation method of the modified metal particles comprises the following steps: (1) Dividing deionized water into two parts, adding metal particles into the first part of deionized water according to a certain proportion, and performing ultrasonic homogenization to form a metal particle dispersion; (2) adding the metal particle dispersion, aniline, and solvent into a reaction container in sequence, and stirring in an ice bath to form a mixed solution; (3) adding an oxidant to the second portion of deionized water and stirring to form an oxidant solution; (4) adding the oxidant solution to the mixed solution, stirring evenly in an ice bath, then heating to room temperature, washing with deionized water, and centrifuging after the washing solution becomes colorless to finally obtain modified metal particles coated with polyaniline on the surface.
6. The acrylic electromagnetic shielding tape according to claim 1, characterized in that: The high acid value polyacrylate adhesive comprises, by weight:
7. The acrylic electromagnetic shielding tape according to claim 6, characterized in that: The initiator is azobisisobutyronitrile, and the solvent is ethyl acetate.
8. The acrylic electromagnetic shielding tape according to claim 6, characterized in that: The preparation method of the high acid value polyacrylate adhesive comprises the following steps: (1) Dividing the solvent into two parts, adding the above-mentioned isooctyl acrylate, 2-hydroxyethyl acrylate, butyl acrylate, acrylic acid, methyl methacrylate and the first part of the solvent into a reaction container in proportion, and stirring at a constant temperature of 80 to 90° C. for 1 to 3 hours in a N2 atmosphere to form a mixed solution; (2) adding the initiator AIBN to the second part of the solvent to prepare an initiator solution according to the above-mentioned number of portions; (3) adding half of the initiator solution to the mixed solution and reacting at 80-90° C. for 1-2 h; (4) adding the remaining initiator solution and reacting at 80-90° C. for another 4-6 hours; (5) cooling to 30-40° C., filtering while hot, and obtaining the high acid value polyacrylate adhesive.
9. The acrylic electromagnetic shielding tape according to any one of claims 1 to 8, characterized in that: The resin is rosin resin, which is dissolved in ethyl acetate to form a resin solution; the curing agent is at least one of toluene diisocyanate, hexamethylene diisocyanate, and 4,4'-dicyclohexylmethane diisocyanate; and the antioxidant is benzotriazole, which is dissolved in ethyl acetate to form an antioxidant solution.
10. A method for preparing the acrylic electromagnetic shielding tape according to any one of claims 1 to 8, characterized in that: The adhesive tape further comprises a substrate layer and a release layer, and the preparation method of the adhesive tape comprises the following steps: (1) adding a high acid value polyacrylate adhesive, a tackifying resin solution, an antioxidant solution, and modified metal particles into a reaction container in proportion and stirring them uniformly to form a mixed solution; (2) adding the curing agent to the mixed solution in proportion, stirring evenly to form a mixture; (3) applying the mixture onto the release layer and then placing it in a drying oven to remove the solvent; (4) taking out the dried adhesive / release layer and pasting it on the substrate layer; (5) Then, the mixture is placed in a drying oven for aging to obtain the acrylic electromagnetic shielding tape.