Acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive, pressure-sensitive adhesive tape and preparation method thereof
By introducing fluorine-containing acrylate monomers and adjusting the monomer ratio in the polyacrylate pressure-sensitive tape, combined with crosslinking agent, the problem of insufficient acid and alkali resistance of polyacrylate pressure-sensitive tape is solved, and high-performance tape preparation is achieved , suitable for electronic product applications in a variety of complex environments.
Patent Information
- Application Number
- CN202411143905.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-12
AI Technical Summary
The existing polyacrylate pressure-sensitive tape has poor acid and alkali resistance in electronic products, and is prone to residual glue, liquid seepage and bubble problems, affecting the protection effect.
The fluorine-containing acrylate monomers are used to participate in the copolymerization, adjust the ratio of acrylate soft monomers and hard monomers, combine with crosslinking agents to prepare acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesives, and pass specific process steps and conditions. Made of acid and alkali resistant polyacrylate pressure sensitive tape.
It significantly improves the acid and alkali resistance and peeling power of pressure-sensitive adhesive tape, avoids degumming, residual glue and liquid leakage during the adhesion and peeling process, and is suitable for electronic products in complex environments.
Smart Images

Figure CN118931436A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of pressure-sensitive adhesive tapes, and in particular to an acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive, a pressure-sensitive adhesive tape and a preparation method thereof. Background Art
[0002] Pressure-sensitive tape refers to a tape that adheres to the surface of the adherend through finger pressure to provide surface protection, so that the adherend can avoid contamination and damage during manufacturing, transportation, and storage. The pressure-sensitive adhesive layer is a viscoelastic body that has both liquid viscosity and solid elasticity. Pressure-sensitive tapes are widely used in packaging, automobiles, transportation, electronics, building materials, machinery, medical care, aerospace, etc. Among them, polyacrylate pressure-sensitive tapes occupy an important position in the field of pressure-sensitive tapes due to their excellent temperature resistance, chemical resistance, and easy availability of raw materials.
[0003] In the fields of electronics, semiconductors, etc., pressure-sensitive tape is an indispensable consumable in process manufacturing, and it needs to meet the requirements of easy adhesion, easy peeling, no residual adhesive, moisture and heat resistance, and temperature resistance. With the development of high-precision and cutting-edge technologies, the requirements for pressure-sensitive tape are getting higher and higher. At present, when pressure-sensitive tape is used in electronic products such as electroplating or chemical plating, it is prone to problems such as residual adhesive and liquid seepage due to its poor acid and alkali resistance. At the same time, it is easy to generate bubbles when it is attached to the adherend, affecting the protection effect. Therefore, it is urgent to develop pressure-sensitive tape that can meet a variety of usage scenarios. Summary of the invention
[0004] The object of the present invention is to provide an acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive, a pressure-sensitive adhesive tape and a preparation method thereof in view of the deficiencies in the prior art.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a method for preparing an acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive, comprising the following steps:
[0007] 1) mixing acrylate soft monomer, acrylate hard monomer, acrylate functional monomer, fluorine-containing acrylate monomer, a first part of thermal initiator and a first part of solvent to obtain a monomer mixed solution;
[0008] 2) reacting the first part of the monomer mixed solution under a nitrogen atmosphere to obtain a reaction intermediate I;
[0009] 3) adding the second part of the monomer mixed solution dropwise to the reaction intermediate I, and reacting after the addition is completed to obtain the reaction intermediate II;
[0010] 4) adding the second part of the thermal initiator dropwise to the reaction intermediate II, and reacting after the addition is completed to obtain an adhesive solution;
[0011] 5) Mixing the second part of the solvent and the adhesive solution to obtain an acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive.
[0012] Preferably, the acrylic acid ester soft monomer comprises one or more of n-butyl acrylate, n-pentyl acrylate, isopentyl acrylate, isooctyl acrylate, 2-ethylhexyl acrylate, 2-nonyl acrylate, isononyl acrylate, decyl acrylate, undecyl acrylate and tridecyl acrylate;
[0013] The acrylic acid ester hard monomer comprises one or more of methyl (meth)acrylate, acrylonitrile, styrene and vinyl acetate;
[0014] The acrylate functional monomer comprises one or more of acrylic acid, itaconic acid, hydroxyethyl acrylate, hydroxypropyl acrylate and glycidyl acrylate;
[0015] The fluorine-containing acrylate monomer comprises one or more of trifluoroethyl (meth)acrylate, hexafluorobutyl (meth)acrylate, heptafluorobutyl acrylate, hexafluoroisopropyl (meth)acrylate, octafluoropentyl (meth)acrylate, dodecafluoroheptyl (meth)acrylate, perfluorodecyl ethyl acrylate, perfluorobutyl ethyl acrylate and perfluoroalkyl ethyl methacrylate;
[0016] The thermal initiator comprises azobisisobutyronitrile and / or dibenzoyl peroxide, and the solvent comprises one or more of ethyl acetate, toluene and butyl acetate.
[0017] Preferably, in step 1), the mass ratio of the acrylate soft monomer, acrylate hard monomer, acrylate functional monomer and fluorine-containing acrylate monomer is 60-70:15-25:5-10:5-35, the mass ratio of the first part of the thermal initiator to the acrylate soft monomer is 0.25-0.45:60-70, and the mass ratio of the first part of the solvent to the acrylate soft monomer is 90-130:60-70.
[0018] Preferably, the mass ratio of the first part thermal initiator to the second part thermal initiator is 6-8:1, the mass ratio of the first part solvent to the second part solvent is 10-12:1, and the mass ratio of the first part monomer mixed solution to the second part monomer mixed solution is 35-45:55-65.
[0019] Preferably, the reaction temperature in step 2) is 70-85°C, and the reaction time is 1-2h; the dropwise addition time in step 3) is 1.5-2.5h, the reaction temperature is 70-85°C, and the reaction time is 1.5-2.5h; the dropwise addition time in step 4) is 0.2-0.8h, the reaction temperature is 70-85°C, and the reaction time is 3-4h.
[0020] Preferably, the solid content of the acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive in step 5) is 35-45%.
[0021] The invention also provides the acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive prepared by the preparation method.
[0022] The present invention also provides a method for preparing an acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive tape comprising the acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive, comprising mixing the acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive with a cross-linking agent to obtain an adhesive mixture; coating the adhesive mixture on a release film, and laminating the mixture with a substrate film after drying to obtain the acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive tape.
[0023] Preferably, the cross-linking agent comprises one or more of aliphatic isocyanate, aromatic isocyanate and multifunctional epoxy resin, and the mass of the cross-linking agent is 1 to 5% of the mass of the acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive; the coating thickness is 10 to 20 μm; the drying temperature is 70 to 90° C., and the drying time is 1 to 2 minutes; the aging temperature is 40 to 50° C., and the aging time is 2 to 4 days.
[0024] The invention also provides an acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive tape prepared by the preparation method.
[0025] The beneficial effects of the present invention include the following:
[0026] 1) In the present invention, fluorinated acrylate monomers participate in copolymerization reactions, and structural units of fluorinated acrylate are introduced into the acrylate polymerization system to form polyacrylate pressure-sensitive adhesives and pressure-sensitive tapes having low surface energy and excellent acid and alkali resistance.
[0027] 2) The present invention adjusts the glass transition temperature of the pressure-sensitive adhesive by adjusting the usage ratio of the acrylate soft monomer and the acrylate hard monomer to adapt to different use environments; and adjusts the usage of the cross-linking agent to achieve the regulation of the gel rate of the pressure-sensitive adhesive, thereby improving its cohesion and temperature resistance.
[0028] 3) The pressure-sensitive adhesive tape of the present invention has a suitable peeling force, can be well attached to semiconductor materials such as silicon, silicon carbide, and gallium nitride and can be easily peeled off, and there is no debonding, residual adhesive, or liquid seepage during the attachment and peeling process. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a schematic structural diagram of the acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive tape of the present invention. DETAILED DESCRIPTION
[0030] The present invention provides a method for preparing an acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive, comprising the following steps:
[0031] 1) mixing acrylate soft monomer, acrylate hard monomer, acrylate functional monomer, fluorine-containing acrylate monomer, a first part of thermal initiator and a first part of solvent to obtain a monomer mixed solution;
[0032] 2) reacting the first part of the monomer mixed solution under a nitrogen atmosphere to obtain a reaction intermediate I;
[0033] 3) adding the second part of the monomer mixed solution dropwise to the reaction intermediate I, and reacting after the addition is completed to obtain the reaction intermediate II;
[0034] 4) adding the second part of the thermal initiator dropwise to the reaction intermediate II, and reacting after the addition is completed to obtain an adhesive solution;
[0035] 5) Mixing the second part of the solvent and the adhesive solution to obtain an acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive.
[0036] In the present invention, the acrylic acid ester soft monomer preferably comprises one or more of n-butyl acrylate, n-pentyl acrylate, isopentyl acrylate, isooctyl acrylate, 2-ethylhexyl acrylate, 2-nonyl acrylate, isononyl acrylate, decyl acrylate, undecyl acrylate and tridecyl acrylate;
[0037] The acrylic acid ester hard monomer preferably comprises one or more of methyl (meth)acrylate, acrylonitrile, styrene and vinyl acetate;
[0038] The acrylate functional monomer preferably comprises one or more of acrylic acid, itaconic acid, hydroxyethyl acrylate, hydroxypropyl acrylate and glycidyl acrylate;
[0039] The fluorine-containing acrylate monomer preferably comprises one or more of trifluoroethyl (meth)acrylate, hexafluorobutyl (meth)acrylate, heptafluorobutyl acrylate, hexafluoroisopropyl (meth)acrylate, octafluoropentyl (meth)acrylate, dodecafluoroheptyl (meth)acrylate, perfluorodecyl ethyl acrylate, perfluorobutyl ethyl acrylate and perfluoroalkyl ethyl methacrylate;
[0040] The thermal initiator preferably comprises azobisisobutyronitrile and / or dibenzoyl peroxide, and the solvent preferably comprises one or more of ethyl acetate, toluene and butyl acetate.
[0041] In the present invention, the mass ratio of the acrylate soft monomer, acrylate hard monomer, acrylate functional monomer and fluorine-containing acrylate monomer in step 1) is preferably 60-70:15-25:5-10:5-35, more preferably 62-68:18-23:6-9:15-30, and more preferably 64-66:20-21:7-8:20-25; the mass ratio of the first part of the thermal initiator to the acrylate soft monomer is preferably 0.25-0.45:60-70, more preferably 0.3-0.4:62-68, and more preferably 0.32-0.35:64-66; the mass ratio of the first part of the solvent to the acrylate soft monomer is preferably 90-130:60-70, more preferably 100-120:62-68, and more preferably 110-115:64-66.
[0042] In the present invention, the mass ratio of the first part of the thermal initiator to the second part of the thermal initiator is preferably 6-8:1, more preferably 6.5-7.5:1, and more preferably 7:1; the mass ratio of the first part of the solvent to the second part of the solvent is preferably 10-12:1, more preferably 10.5-11.5:1, and more preferably 11:1; the mass ratio of the first part of the monomer mixed solution to the second part of the monomer mixed solution is preferably 35-45:55-65, more preferably 37-43:57-63, and more preferably 40:60.
[0043] In the present invention, the reaction in step 1) is preferably timed from the time when condensation reflux occurs.
[0044] In the present invention, the reaction temperature in step 2) is preferably 70-85°C, more preferably 75-80°C; the reaction time is preferably 1-2h, more preferably 1.5h; the dropwise addition time in step 3) is preferably 1.5-2.5h, more preferably 2h; the reaction temperature is preferably 70-85°C, more preferably 75-80°C; the reaction time is preferably 1.5-2.5h, more preferably 2h; the dropwise addition time in step 4) is preferably 0.2-0.8h, more preferably 0.5h; the reaction temperature is preferably 70-85°C, more preferably 75-80°C; the reaction time is preferably 3-4h, more preferably 3.5h.
[0045] In the present invention, the solid content of the acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive in step 5) is preferably 35-45%, more preferably 38-43%, and more preferably 40%.
[0046] The invention also provides the acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive prepared by the preparation method.
[0047] The present invention also provides a method for preparing an acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive tape comprising the acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive, comprising mixing the acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive with a cross-linking agent to obtain an adhesive mixture; coating the adhesive mixture on a release film, and laminating the mixture with a substrate film after drying to obtain the acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive tape.
[0048] In the present invention, the cross-linking agent preferably comprises one or more of aliphatic isocyanate, aromatic isocyanate and multifunctional epoxy resin, and the mass of the cross-linking agent is preferably 1-5% of the mass of the acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive, more preferably 2-4%, and more preferably 2.02%; the coating thickness is preferably 10-20 μm, more preferably 13-18 μm, and more preferably 15 μm; the drying temperature is preferably 70-90°C, more preferably 75-85°C, and more preferably 80°C; the drying time is preferably 1-2 min, more preferably 1.3-1.8 min, and more preferably 1.5 min; the aging temperature is preferably 40-50°C, more preferably 43-48°C, and more preferably 45°C; the aging time is preferably 2-4 days, and more preferably 3 days.
[0049] The present invention also provides an acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive tape prepared by a preparation method of the acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive tape comprising the acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive.
[0050] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0051] Example 1
[0052] 40g of n-butyl acrylate, 20g of isooctyl acrylate, 10g of methyl (meth)acrylate, 10g of vinyl acetate, 10g of hydroxyethyl acrylate, 5g of trifluoroethyl (meth)acrylate, 0.35g of azobisisobutyronitrile and 110g of ethyl acetate were mixed to obtain a monomer mixed solution. 40% of the total mass of the monomer mixed solution was poured into a reactor, the reactor was heated to 75°C, nitrogen was introduced and stirring was started, and the timing was started when condensation reflux appeared in the reactor, and the reaction was carried out for 2h.
[0053] The remaining monomer mixed solution was added dropwise to the reactor for 2 hours. The reactor was heated to 80°C and kept warm for 2 hours after the addition was completed.
[0054] 0.05 g of azobisisobutyronitrile was added dropwise to the reaction kettle for 0.5 h. After the addition was completed, the reaction was kept warm at 80° C. for 4 h.
[0055] 10 g of ethyl acetate was added into the reaction kettle and cooled naturally to obtain an acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive having a solid content of 38%.
[0056] The acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive is mixed with the isocyanate crosslinking agent MDI and the epoxy resin crosslinking agent AG80 (the mass of the isocyanate crosslinking agent is 2% of the mass of the acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive, and the mass of the epoxy resin crosslinking agent is 0.02% of the mass of the acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive) to obtain an adhesive mixture. The adhesive mixture is coated on a polyethylene terephthalate release film with a coating thickness of 15 μm, dried at 80° C. for 1.5 minutes, and then laminated with a polyvinyl chloride substrate film and aged at 45° C. for 3 days to obtain an acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive tape.
[0057] Example 2
[0058] 40 g of n-butyl acrylate, 20 g of isooctyl acrylate, 10 g of methyl (meth)acrylate, 10 g of vinyl acetate, 10 g of hydroxyethyl acrylate, 15 g of trifluoroethyl (meth)acrylate, 0.35 g of azobisisobutyronitrile and 110 g of ethyl acetate were mixed to obtain a monomer mixed solution. 40% of the total mass of the monomer mixed solution was poured into a reactor, the reactor was heated to 75° C., nitrogen was introduced and stirring was started, and the timing was started when condensation reflux appeared in the reactor, and the reaction was carried out for 2 hours.
[0059] The remaining monomer mixed solution was added dropwise to the reactor for 2 hours. The reactor was heated to 80°C and kept warm for 2 hours after the addition was completed.
[0060] 0.05 g of azobisisobutyronitrile was added dropwise to the reaction kettle for 0.5 h. After the addition was completed, the reaction was kept warm at 80° C. for 4 h.
[0061] 10 g of ethyl acetate was added into the reaction kettle and cooled naturally to obtain an acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive having a solid content of 40%.
[0062] The acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive is mixed with the isocyanate crosslinking agent MDI (the mass of the isocyanate crosslinking agent is 2% of the mass of the acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive) to obtain an adhesive mixture. The adhesive mixture is coated on a polyethylene terephthalate release film with a coating thickness of 15 μm, dried at 80° C. for 1.5 minutes, and then laminated with a polyvinyl chloride substrate film and aged at 45° C. for 3 days to obtain an acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive tape.
[0063] Example 3
[0064] 40 g of n-butyl acrylate, 20 g of isooctyl acrylate, 10 g of methyl (meth)acrylate, 10 g of vinyl acetate, 10 g of hydroxyethyl acrylate, 30 g of hexafluorobutyl (meth)acrylate, 0.35 g of azobisisobutyronitrile and 110 g of ethyl acetate were mixed to obtain a monomer mixed solution. 40% of the total mass of the monomer mixed solution was poured into a reactor, the reactor was heated to 75° C., nitrogen was introduced and stirring was started, and the timing was started when condensation reflux appeared in the reactor, and the reaction was carried out for 2 hours.
[0065] The remaining monomer mixed solution was added dropwise to the reactor for 2 hours. The reactor was heated to 80°C and kept warm for 2 hours after the addition was completed.
[0066] 0.05 g of azobisisobutyronitrile was added dropwise to the reaction kettle for 0.5 h. After the addition was completed, the reaction was kept warm at 80° C. for 4 h.
[0067] 10 g of ethyl acetate was added into the reaction kettle and cooled naturally to obtain an acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive having a solid content of 43%.
[0068] The acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive is mixed with the isocyanate crosslinking agent MDI (the mass of the isocyanate crosslinking agent is 2% of the mass of the acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive) to obtain an adhesive mixture. The adhesive mixture is coated on a polyethylene terephthalate release film with a coating thickness of 15 μm, dried at 80° C. for 1.5 minutes, and then laminated with a polyvinyl chloride substrate film and aged at 45° C. for 3 days to obtain an acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive tape.
[0069] Example 4
[0070] 40 g of n-butyl acrylate, 20 g of isooctyl acrylate, 10 g of methyl (meth)acrylate, 10 g of vinyl acetate, 10 g of hydroxyethyl acrylate, 35 g of dodecafluoroheptyl (meth)acrylate, 0.35 g of azobisisobutyronitrile and 110 g of ethyl acetate were mixed to obtain a monomer mixed solution. 40% of the total mass of the monomer mixed solution was poured into a reactor, the reactor was heated to 75° C., nitrogen was introduced and stirring was started, and the timing was started when condensation reflux appeared in the reactor, and the reaction was carried out for 2 hours.
[0071] The remaining monomer mixed solution was added dropwise to the reactor for 2 hours. The reactor was heated to 80°C and kept warm for 2 hours after the addition was completed.
[0072] 0.05 g of azobisisobutyronitrile was added dropwise to the reaction kettle for 0.5 h. After the addition was completed, the reaction was kept warm at 80° C. for 4 h.
[0073] 10 g of ethyl acetate was added into the reaction kettle and cooled naturally to obtain an acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive having a solid content of 45%.
[0074] The acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive is mixed with the isocyanate crosslinking agent MDI (the mass of the isocyanate crosslinking agent is 2% of the mass of the acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive) to obtain an adhesive mixture. The adhesive mixture is coated on a polyethylene terephthalate release film with a coating thickness of 15 μm, dried at 80° C. for 1.5 minutes, and then laminated with a polyvinyl chloride substrate film and aged at 45° C. for 3 days to obtain an acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive tape.
[0075] Example 5
[0076] 35 g of isoamyl acrylate, 33 g of decyl acrylate, 9 g of acrylonitrile, 6 g of vinyl acetate, 6 g of itaconic acid, 20 g of octafluoropentyl (meth)acrylate, 0.3 g of azobisisobutyronitrile and 100 g of butyl acetate were mixed to obtain a monomer mixed solution. 43% of the total mass of the monomer mixed solution was poured into a reactor, the reactor was heated to 70° C., nitrogen was introduced and stirring was started, and the timing was started when condensation reflux appeared in the reactor, and the reaction was carried out for 1 hour.
[0077] The remaining monomer mixed solution was added dropwise to the reactor for 1.5 hours. The reactor was heated to 75°C and kept warm for 1.5 hours after the addition was completed.
[0078] 0.05 g of azobisisobutyronitrile was added dropwise to the reaction kettle for 0.2 h. After the addition was completed, the reaction was kept warm at 75°C for 3 h.
[0079] 8.7 g of butyl acetate was added into the reaction kettle and cooled naturally to obtain an acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive having a solid content of 35%.
[0080] The acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive was mixed with the epoxy resin crosslinker AG80 (the mass of the epoxy resin crosslinker was 4% of the mass of the acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive) to obtain an adhesive mixture. The adhesive mixture was coated on a polyethylene terephthalate release film with a coating thickness of 13 μm, dried at 75° C. for 1.8 min, and then laminated with a polyvinyl chloride substrate film and aged at 43° C. for 4 days to obtain an acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive tape.
[0081] Example 6
[0082] 30 g of 2-ethylhexyl acrylate, 34 g of undecyl acrylate, 12 g of acrylonitrile, 11 g of styrene, 8 g of glycidyl acrylate, 25 g of perfluorodecyl ethyl acrylate, 0.4 g of dibenzoyl peroxide and 130 g of toluene were mixed to obtain a monomer mixed solution. 37% of the total mass of the monomer mixed solution was poured into a reactor, which was heated to 80° C., nitrogen was introduced and stirring was started. When condensation reflux appeared in the reactor, the timing was started and the reaction was carried out for 1.5 hours.
[0083] The remaining monomer mixed solution was added dropwise to the reactor for 2.5 hours. The reactor was heated to 85°C and kept warm for 2.5 hours after the addition was completed.
[0084] 0.05 dibenzoyl peroxide was added dropwise to the reactor for 0.8 h. After the addition was completed, the reaction was kept warm at 85°C for 3.5 h.
[0085] 12.4 g of toluene was added into the reaction kettle and cooled naturally to obtain an acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive having a solid content of 40%.
[0086] The acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive is mixed with the isocyanate crosslinking agent MDI (the mass of the isocyanate crosslinking agent is 1% of the mass of the acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive) to obtain an adhesive mixture. The adhesive mixture is coated on a polyethylene terephthalate release film with a coating thickness of 18 μm, dried at 85° C. for 1.3 minutes, and then laminated with a polyvinyl chloride substrate film and aged at 485° C. for 2 days to obtain an acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive tape.
[0087] Comparative Example 1
[0088] 40 g of butyl acrylate, 20 g of isooctyl acrylate, 10 g of methyl (meth)acrylate, 10 g of vinyl acetate, 10 g of hydroxyethyl acrylate, 0.35 g of azobisisobutyronitrile and 110 g of ethyl acetate were mixed to obtain a monomer mixed solution. 40% of the total mass of the monomer mixed solution was poured into a reactor, the reactor was heated to 75° C., nitrogen was introduced and stirring was started, and the timing was started when condensation reflux appeared in the reactor, and the reaction was carried out for 2 hours.
[0089] The remaining monomer mixed solution was added dropwise to the reactor for 2 hours. The reactor was heated to 80°C and kept warm for 2 hours after the addition was completed.
[0090] 0.05 g of azobisisobutyronitrile was added dropwise to the reaction kettle for 0.5 h. After the addition was completed, the reaction was kept warm at 80° C. for 4 h.
[0091] 10 g of ethyl acetate was added into the reaction kettle and cooled naturally to obtain an acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive having a solid content of 35%.
[0092] The acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive is mixed with the isocyanate crosslinking agent MDI and the epoxy resin crosslinking agent AG80 (the mass of the isocyanate crosslinking agent is 2% of the mass of the acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive, and the mass of the epoxy resin crosslinking agent is 0.02% of the mass of the acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive) to obtain an adhesive mixture. The adhesive mixture is coated on a polyethylene terephthalate release film with a coating thickness of 15 μm, dried at 80° C. for 1.5 minutes, and then laminated with a polyvinyl chloride substrate film and aged at 45° C. for 3 days to obtain an acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive tape.
[0093] 25 mm×30 cm pressure-sensitive adhesive tape samples were cut from the acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive tapes prepared in Examples 1 to 4 and Comparative Example 1, respectively.
[0094] The pressure-sensitive tape samples were attached to 304 standard stainless steel plates and the peeling force test was carried out according to GB / T2792-1998. The test results are shown in Table 1.
[0095] The pressure-sensitive tape sample was attached to the mirror surface of a 500μm silicon wafer and immersed in a sulfuric acid solution with a pH of 1.0 and a sodium hydroxide solution with a pH of 10.0 for 30 minutes, respectively. After being taken out, it was observed whether there were defects such as bubbles, seepage, and debonding. The peeling force test was carried out in accordance with GB / T2792-1998. The test results are shown in Table 1.
[0096] Table 1 Test results of peeling force and acid and alkali resistance of pressure-sensitive adhesive tape
[0097]
[0098]
[0099] As can be seen from Table 1, the present invention introduces a fluorinated acrylate monomer to prepare a monomer mixed solution, and by adding the monomer mixed solution, a thermal initiator and a solvent step by step, and reasonably controlling the mass ratio of each step, each raw material can fully react under better process parameters, the peeling force of the obtained pressure-sensitive adhesive tape is increased, and the acid and alkali resistance is significantly improved, and it can be applied to the field of electronic products in various complex environments such as electroplating or chemical plating.
[0100] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing an acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive, characterized in that: The following steps are included: 1) mixing acrylate soft monomer, acrylate hard monomer, acrylate functional monomer, fluorine-containing acrylate monomer, a first part of thermal initiator and a first part of solvent to obtain a monomer mixed solution; 2) reacting the first part of the monomer mixed solution under a nitrogen atmosphere to obtain a reaction intermediate I; 3) adding the second part of the monomer mixed solution dropwise to the reaction intermediate I, and reacting after the addition is completed to obtain the reaction intermediate II; 4) adding the second part of the thermal initiator dropwise to the reaction intermediate II, and reacting after the addition is completed to obtain an adhesive solution; 5) Mixing the second part of the solvent and the adhesive solution to obtain an acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive.
2. The preparation method according to claim 1, characterized in that: The acrylic acid ester soft monomer comprises one or more of n-butyl acrylate, n-pentyl acrylate, isopentyl acrylate, isooctyl acrylate, 2-ethylhexyl acrylate, 2-nonyl acrylate, isononyl acrylate, decyl acrylate, undecyl acrylate and tridecyl acrylate; The acrylic acid ester hard monomer comprises one or more of methyl (meth)acrylate, acrylonitrile, styrene and vinyl acetate; The acrylate functional monomer comprises one or more of acrylic acid, itaconic acid, hydroxyethyl acrylate, hydroxypropyl acrylate and glycidyl acrylate; The fluorine-containing acrylate monomer comprises one or more of trifluoroethyl (meth)acrylate, hexafluorobutyl (meth)acrylate, heptafluorobutyl acrylate, hexafluoroisopropyl (meth)acrylate, octafluoropentyl (meth)acrylate, dodecafluoroheptyl (meth)acrylate, perfluorodecyl ethyl acrylate, perfluorobutyl ethyl acrylate and perfluoroalkyl ethyl methacrylate; The thermal initiator comprises azobisisobutyronitrile and / or dibenzoyl peroxide, and the solvent comprises one or more of ethyl acetate, toluene and butyl acetate.
3. The preparation method according to claim 1 or 2, characterized in that: In step 1), the mass ratio of the acrylate soft monomer, acrylate hard monomer, acrylate functional monomer and fluorine-containing acrylate monomer is 60-70:15-25:5-10:5-35, the mass ratio of the first part of thermal initiator to the acrylate soft monomer is 0.25-0.45:60-70, and the mass ratio of the first part of solvent to the acrylate soft monomer is 90-130:60-70.
4. The preparation method according to claim 3, characterized in that: The mass ratio of the first part of thermal initiator to the second part of thermal initiator is 6-8:1, the mass ratio of the first part of solvent to the second part of solvent is 10-12:1, and the mass ratio of the first part of monomer mixed solution to the second part of monomer mixed solution is 35-45:55-65.
5. The preparation method according to claim 4, characterized in that: The reaction temperature of step 2) is 70-85°C, and the reaction time is 1-2h; the dropwise addition time of step 3) is 1.5-2.5h, the reaction temperature is 70-85°C, and the reaction time is 1.5-2.5h; the dropwise addition time of step 4) is 0.2-0.8h, the reaction temperature is 70-85°C, and the reaction time is 3-4h.
6. The preparation method according to claim 4 or 5, characterized in that: Step 5) The solid content of the acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive is 35-45%.
7. The acid- and alkali-resistant polyacrylate pressure-sensitive adhesive prepared by the preparation method according to any one of claims 1 to 6.
8. A method for preparing an acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive tape comprising the acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive according to claim 7, characterized in that: The acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive is mixed with a cross-linking agent to obtain an adhesive mixture; the adhesive mixture is coated on a release film, and after drying, it is laminated with a substrate film for aging to obtain an acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive tape.
9. The preparation method according to claim 8, characterized in that: The cross-linking agent comprises one or more of aliphatic isocyanate, aromatic isocyanate and multifunctional epoxy resin, and the mass of the cross-linking agent is 1-5% of the mass of the acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive; the coating thickness is 10-20 μm; the drying temperature is 70-90° C., and the drying time is 1-2 minutes; the aging temperature is 40-50° C., and the aging time is 2-4 days.
10. The acid-resistant and alkali-resistant polyacrylate pressure-sensitive adhesive tape prepared by the preparation method according to claim 8 or 9.
Citation Information
Cited By
Waterproof pressure-sensitive adhesive tape and production process thereof
CN120059624A