Yellowing-resistant transparent flame-retardant epoxy resin adhesive and preparation method thereof
This yellowing-resistant, transparent, flame-retardant epoxy resin adhesive, prepared using specific components and processes, solves the problems of insufficient transparency and flame retardancy in existing epoxy resin adhesives. It achieves high transparency, yellowing resistance, and excellent flame retardancy, making it suitable for potting materials for electronic and electrical components.
Patent Information
- Application Number
- CN202411243234.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-12
AI Technical Summary
Existing epoxy resin adhesives suffer from poor transparency, yellowing, and insufficient flame retardancy in the electronics and electrical fields, failing to meet the high requirements of potting materials.
A yellowing-resistant, transparent, flame-retardant epoxy resin adhesive is prepared by using a specific ratio of epoxy resin, alicyclic epoxy resin, liquid acid anhydride, DOPO flame retardant, antioxidant, ultraviolet light absorber, and accelerator through a mixing and curing process.
It improves the transparency and yellowing resistance of adhesives, enhances flame retardancy, resists UV erosion, extends product life, adapts to complex stress environments, and maintains color stability.
Smart Images

Figure CN118931451A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and particularly relates to a yellowing-resistant transparent flame-retardant epoxy resin adhesive and a preparation method thereof. Background Art
[0002] With the rapid development of epoxy resin adhesives, epoxy resins are widely used in electricity, electronics, information, aerospace, construction and sports goods due to their excellent electrical properties, high temperature resistance, solvent resistance, acid and alkali resistance, good adhesion, light weight and low cost. Higher requirements are also put forward for epoxy resins used for potting. In addition to requiring good transparency and insulation properties, higher requirements are also put forward for its fire resistance and yellowing resistance. Preventing short circuits and fires in electrical component potting glue puts forward new requirements for the flame retardancy of resins, such as the UL-94 fire test, which must meet the V-0 regulations. Based on this, an epoxy + anhydride system adhesive is developed to meet the above transparency, yellowing resistance, flame retardancy, mechanical properties and electrical properties of epoxy resin adhesives and preparation methods.
[0003] The existing solvent-free epoxy adhesive technology has the following problems: amines and liquid acid anhydrides are used as curing agents, and the resin cured product is yellow to brown and other colors, which cannot meet the requirements of colorless and transparent potting resin in the electronic and electrical fields; during use, environmental erosion such as heat and ultraviolet light will cause the resin cured product to turn yellow and age, resulting in a decrease in the electrical and mechanical properties of the resin cured product; when encapsulating electronic and electrical components, traditional epoxy adhesives have a low oxygen index and are flammable and combustible, which cannot meet the components' requirements for flame retardancy. Summary of the invention
[0004] In order to overcome the above-mentioned shortcomings of the prior art, the object of the present invention is to provide a yellowing-resistant transparent flame-retardant epoxy resin adhesive and a preparation method thereof.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] In a first aspect, the present invention provides a yellowing-resistant, transparent, flame-retardant epoxy resin adhesive, which comprises, by weight, 7 to 9 parts of epoxy resin, 1 to 3 parts of alicyclic epoxy resin, 7 to 9.5 parts of liquid acid anhydride, 1 to 2 parts of epoxy reactive toughening agent, 0.8 to 1.5 parts of DOPO flame retardant, 0.1 to 0.5 parts of antioxidant, 0.1 to 0.5 parts of ultraviolet light absorber and 0.01 to 1 parts of accelerator.
[0007] Preferably, the epoxy resin is one or more of bisphenol A epoxy resin, bisphenol F epoxy resin and hydrogenated epoxy resin.
[0008] Preferably, the alicyclic epoxy resin is one or more of 3,4-epoxycyclohexylcarboxylic acid-3',4'-epoxycyclohexyl methyl ester, bis((3,4-epoxycyclohexyl)methyl)adipate, poly[(2-oxiranyl)-1,2-cyclohexanediol]2-ethyl-2-(hydroxymethyl)-1,3-propylene glycol ether (3:1) and 3,4-epoxycyclohexyl methyl methacrylate.
[0009] Preferably, the liquid acid anhydride is one or more of methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride and methylnadic anhydride.
[0010] Preferably, the epoxy-reactive toughening agent is one or more of a long-chain linear hydroxyl functional polyether compound and a long-chain aliphatic compound.
[0011] Preferably, the DOPO flame retardant is 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide.
[0012] Preferably, the antioxidant is one or more of 2,6-di-tert-butyl-p-cresol, phosphite antioxidants, hindered phenol antioxidants and pentaerythritol diphosphite antioxidants.
[0013] Preferably, the ultraviolet light absorber is a liquid ultraviolet light absorber; and the accelerator is one or more of BDMA, modified imidazoles, DBU salts and modified phosphorus accelerators.
[0014] In a second aspect, the present invention provides a method for preparing a yellowing-resistant transparent flame-retardant epoxy resin adhesive, comprising the following steps:
[0015] S1: mixing an epoxy resin and an alicyclic epoxy resin and dispersing them uniformly to obtain an epoxy resin mixture;
[0016] S2: mixing liquid acid anhydride, epoxy active toughening agent, DOPO flame retardant, antioxidant, ultraviolet light absorber and accelerator together and dispersing them evenly to prepare epoxy resin curing agent;
[0017] S3: The epoxy resin mixture and the epoxy resin curing agent are mixed in a mass ratio of 1:(0.7-1.3) to obtain a yellowing-resistant transparent flame-retardant epoxy resin adhesive.
[0018] Preferably, S2 comprises the following steps:
[0019] S21: heating the liquid acid anhydride to 60° C.-80° C., adding the DOPO flame retardant under stirring, and stirring at the same temperature until the DOPO flame retardant melts to form a mixed liquid;
[0020] S22: Cool the mixed solution to below 50° C., add epoxy active toughening agent, antioxidant and ultraviolet light absorber under stirring, and add accelerator after reacting for 50 to 70 minutes to obtain epoxy resin curing agent.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] The epoxy resin adhesive of the present invention has extremely high transparency, and the light transmittance reaches ≥88%, which is significantly better than the existing epoxy anhydride system resin used in the electrical and electronic fields; by adding an ultraviolet light absorber, the adhesive of the present invention can effectively resist the erosion of ultraviolet rays, slow down the aging phenomenon caused by ultraviolet light irradiation, protect electronic components from environmental factors, and improve the reliability and durability of the product; by adding an epoxy active toughening agent, the toughness of the adhesive is effectively improved, so that it can better adapt to various complex stress environments during use, and reduce cracking or breakage caused by stress concentration; the combination ratio of different substances enables the present invention to effectively improve the high temperature yellowing resistance, can maintain color stability for a long time at a high temperature, and extend the service life of the product. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The present invention is a schematic flow chart of a method for preparing a yellowing-resistant, transparent, flame-retardant epoxy resin adhesive;
[0024] Figure 2 Schematic diagram of light transmittance of the yellowing-resistant, transparent, flame-retardant epoxy resin adhesive prepared in Examples 2 and 6 of the present invention. DETAILED DESCRIPTION
[0025] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0026] It should be understood that when used in this specification and the appended claims, the terms "include" and "comprises" indicate the presence of described features, integers, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or combinations thereof.
[0027] It should also be understood that the terms used in the present specification are only for the purpose of describing specific embodiments and are not intended to limit the present invention. As used in the present specification and the appended claims, unless the context clearly indicates otherwise, the singular forms "a", "an" and "the" are intended to include plural forms.
[0028] It should be further understood that the term "and / or" used in the present description and the appended claims refers to any and all possible combinations of one or more of the associated listed items, and includes these combinations.
[0029] Various structural schematic diagrams of the embodiments disclosed in the present invention are shown in the accompanying drawings. These figures are not drawn to scale, and some details are magnified and some details may be omitted for the purpose of clear expression. The shapes of various regions and layers shown in the figures and the relative sizes and positional relationships therebetween are only exemplary, and may deviate in practice due to manufacturing tolerances or technical limitations, and those skilled in the art may additionally design regions / layers with different shapes, sizes, and relative positions according to actual needs.
[0030] The first object of the present invention is to provide a yellowing-resistant transparent flame-retardant epoxy resin adhesive, which comprises, by weight, 7 to 9 parts of epoxy resin, 1 to 3 parts of alicyclic epoxy resin, 7 to 9.5 parts of liquid acid anhydride, 1 to 2 parts of epoxy reactive toughening agent, 0.8 to 1.5 parts of DOPO flame retardant, 0.1 to 0.5 parts of antioxidant, 0.1 to 0.5 parts of ultraviolet light absorber and 0.01 to 1 parts of accelerator. The epoxy resin provided by the present invention has high transparency, such as Figure 2 , which is a schematic diagram of the light transmittance of the yellowing-resistant transparent flame-retardant epoxy resin adhesive prepared in Example 2 and Example 6 of the present invention, Figure 2 It can be seen that its light transmittance is ≥88%, which is a great improvement on the existing epoxy anhydride system resin used in the electrical and electronic fields. Due to the addition of DOPO flame retardant, the adhesive has excellent flame retardant properties. With the increase of flame retardant, its carbonization effect is more obvious and the flame retardant effect is better. It is more excellent in high temperature yellowing resistance and ultraviolet light aging performance. In view of the above properties, it can be used for potting and pouring of electrical and electronic components.
[0031] Among them, the epoxy resin is one or more of bisphenol A epoxy resin, bisphenol F epoxy resin and hydrogenated epoxy resin. The alicyclic epoxy resin is one or more of 3,4-epoxycyclohexylcarboxylic acid-3',4'-epoxycyclohexyl methyl ester, bis((3,4-epoxycyclohexyl)methyl) adipate, poly[(2-oxirane)-1,2-cyclohexanediol]2-ethyl-2-(hydroxymethyl)-1,3-propylene glycol ether (3:1) and 3,4-epoxycyclohexyl methyl methacrylate. The liquid anhydride is one or more of methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride and methylnadic anhydride. The epoxy active toughening agent is one or more of a long-chain linear hydroxyl functional group polyether compound and a long-chain aliphatic compound. The DOPO flame retardant is 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide. The antioxidant is one or more of 2,6-di-tert-butyl-p-cresol, phosphite antioxidants, hindered phenol antioxidants, and pentaerythritol diphosphite antioxidants. The ultraviolet light absorber is a liquid ultraviolet light absorber; and the accelerator is one or more of BDMA, modified imidazoles, DBU salts, and modified phosphorus accelerators.
[0032] The second object of the present invention is to provide a method for preparing a yellowing-resistant transparent flame-retardant epoxy resin adhesive. Figure 1 As shown, the following steps are included:
[0033] S1: mixing an epoxy resin and an alicyclic epoxy resin and dispersing them uniformly to obtain an epoxy resin mixture;
[0034] S2: mixing liquid acid anhydride, epoxy active toughening agent, DOPO flame retardant, antioxidant, ultraviolet light absorber and accelerator together and dispersing them evenly to prepare epoxy resin curing agent;
[0035] S3: Mix the epoxy resin mixture and the epoxy resin curing agent in a mass ratio of 1: (0.7-1.3), control the gelation time at 180″-210″ / 160°C, and obtain a yellowing-resistant transparent flame-retardant epoxy resin adhesive after mixing, and obtain a transparent resin cured product according to the following curing conditions. Among them, the initial curing conditions: temperature is 60-90°C, preferably 75-80°C, and the time is 2-4h; the intermediate curing conditions: temperature is 100-120°C, preferably 110-120°C, and the time is 2-4h; the final curing conditions: temperature is 140-160°C, preferably 140-150°C, and the time is 8-10h. For example, curing can be carried out according to the following process: curing at 80°C for 2h-4h, then curing at 120°C for 2h-4h, and finally curing at 140°C for 8h-10h.
[0036] Wherein, S2 includes the following steps:
[0037] S21: heating the liquid acid anhydride to 60° C.-80° C., adding the DOPO flame retardant under stirring, and stirring at the same temperature until the DOPO flame retardant melts to form a mixed liquid;
[0038] S22: Cool the mixed solution to below 50° C., add epoxy active toughening agent, antioxidant and ultraviolet light absorber under stirring, and add accelerator after reacting for 50 to 70 minutes to obtain epoxy resin curing agent.
[0039] The present invention can also store the epoxy resin mixture and the epoxy resin curing agent separately. When in use, the epoxy resin mixture and the epoxy resin curing agent are mixed at a mass ratio of 1: (0.7-1.3), stirred evenly, and poured on the components to be encapsulated in a normal or vacuum state. The gel time is usually controlled to be 180"-210" at 160°C, and then cured according to the above-mentioned curing process to obtain the desired performance.
[0040] The method provided by the invention is simple and easy to implement, has a wide range of material sources, is low in cost and has good use effect.
[0041] Example 1
[0042] 8 parts of bisphenol A epoxy resin and 2 parts of 3,4-epoxycyclohexylcarboxylic acid-3',4'-epoxycyclohexyl methyl ester were added into a reaction kettle and dispersed evenly to prepare an epoxy resin mixture for standby use; 8.6 parts of methyltetrahydrophthalic anhydride were heated to 60°C, 1.5 parts of DOPO flame retardant were added under stirring, and the mixture was stirred and kept warm until the DOPO flame retardant melted to form a mixed liquid, and the mixed liquid was cooled to below 50°C, 1 part of a long-chain linear hydroxyl functional group polyether compound, 0.2 parts of a phosphite antioxidant, and 0.5 parts of a liquid ultraviolet light absorber were added under stirring, and after reacting for 60 minutes, 0.01 parts of a DBU salt accelerator were added to prepare a curing agent.
[0043] 1 part of epoxy resin mixture and 0.7 part of curing agent are mixed evenly in proportion, and the gel time is 180" at 160°C; then, it is cured at 80°C for 2h, then at 120°C for 2h, and finally at 140°C for 8h to obtain a yellowing-resistant transparent flame-retardant epoxy resin cured product.
[0044] Example 2
[0045] 8 parts of bisphenol A epoxy resin and 2 parts of bis((3,4-epoxycyclohexyl)methyl)adipate were added into a reaction kettle and dispersed evenly to prepare an epoxy resin mixture for standby use; 8.6 parts of methylhexahydrophthalic anhydride were heated to 65°C, 1.5 parts of DOPO flame retardant were added under stirring, and the mixture was stirred and kept warm until the DOPO flame retardant melted to form a mixed liquid, and the mixed liquid was cooled to below 50°C, 1 part of a long-chain linear hydroxyl functional group polyether compound, 0.2 parts of a phosphite antioxidant, and 0.5 parts of a liquid ultraviolet light absorber were added under stirring, and after reacting for 60 minutes, 0.01 parts of a DBU salt accelerator were added to prepare a curing agent.
[0046] 1 part of epoxy resin mixture and 0.8 part of curing agent were mixed evenly in proportion, the gel time was 190" at 160°C, cured at 75°C for 4h, then cured at 100°C for 4h, and finally cured at 140°C for 10h to obtain a yellowing-resistant transparent flame-retardant epoxy resin cured product.
[0047] Example 3
[0048] 8 parts of bisphenol F epoxy resin and 2 parts of 3,4-epoxycyclohexylcarboxylic acid-3',4'-epoxycyclohexyl methyl ester were added into a reaction kettle and dispersed evenly to prepare an epoxy resin mixture for standby use; 8.6 parts of methyltetrahydrophthalic anhydride were heated to 70°C, 0.8 parts of DOPO flame retardant were added under stirring, and the mixture was stirred and kept warm until the DOPO flame retardant melted to form a mixed liquid, and the mixed liquid was cooled to below 50°C, 1 part of a long-chain linear hydroxyl functional group polyether compound, 0.5 parts of a phosphite antioxidant, and 0.3 parts of a liquid ultraviolet light absorber were added under stirring, and after reacting for 70 minutes, 0.01 parts of a modified phosphorus accelerator were added to prepare a curing agent.
[0049] 1 part of epoxy resin mixture and 0.9 part of curing agent are mixed evenly in proportion, the gel time is 200" at 160°C, cured at 60°C for 4h, then cured at 110°C for 3h, and finally cured at 160°C for 8h to obtain yellowing-resistant transparent flame-retardant epoxy resin cured product.
[0050] Example 4
[0051] 8 parts of bisphenol F epoxy resin and 2 parts of bis((3,4-epoxycyclohexyl)methyl)adipate were added into a reaction kettle and dispersed evenly to prepare an epoxy resin mixture for standby use; 8.6 parts of methyltetrahydrophthalic anhydride were heated to 75°C, 0.8 parts of DOPO flame retardant were added under stirring, and the mixture was stirred and kept warm until the DOPO flame retardant melted to form a mixed liquid, and the mixed liquid was cooled to below 50°C, 1 part of a long-chain linear hydroxyl functional group polyether compound, 0.5 parts of a phosphite antioxidant, and 0.3 parts of a liquid ultraviolet light absorber were added under stirring, and after reacting for 70 minutes, 0.01 parts of a modified phosphorus accelerator were added to prepare a curing agent.
[0052] One part of epoxy resin mixture and one part of curing agent were mixed evenly in proportion, the gel time was 210" at 160°C, cured at 90°C for 2h, then cured at 115°C for 3h, and finally cured at 150°C for 9h to obtain a yellowing-resistant transparent flame-retardant epoxy resin cured product.
[0053] Example 5
[0054] 8 parts of hydrogenated epoxy resin and 2 parts of poly[(2-oxirane)-1,2-cyclohexanediol]2-ethyl-2-(hydroxymethyl)-1,3-propylene glycol ether (3:1) were added into a reaction kettle and dispersed evenly to prepare an epoxy resin mixture for standby use; 8.6 parts of methyltetrahydrophthalic anhydride were heated to 80°C, 1.3 parts of DOPO flame retardant were added under stirring, and the mixture was stirred and kept warm until the DOPO flame retardant melted to form a mixed solution, and the mixed solution was cooled to below 50°C, 1 part of a long-chain aliphatic compound, 0.2 parts of a phosphite antioxidant, and 0.2 parts of a liquid ultraviolet light absorber were added under stirring, and after reacting for 70 minutes, 0.02 parts of a modified imidazole accelerator were added to prepare a curing agent.
[0055] 1 part of epoxy resin mixture and 1.1 parts of curing agent were mixed evenly in proportion, the gel time was 205" at 160°C, cured at 85°C for 3h, then cured at 105°C for 3h, and finally cured at 145°C for 9h to obtain yellowing-resistant transparent flame-retardant epoxy resin cured product.
[0056] Example 6
[0057] 8 parts of hydrogenated epoxy resin and 2 parts of poly[(2-oxirane)-1,2-cyclohexanediol]2-ethyl-2-(hydroxymethyl)-1,3-propylene glycol ether (3:1) were added into a reaction kettle and dispersed evenly to prepare an epoxy resin mixture for standby use; 8.6 parts of methyl hexahydrophthalic anhydride were heated to 80°C, 1.3 parts of DOPO flame retardant were added under stirring, and the mixture was stirred and kept warm until the DOPO flame retardant melted to form a mixed solution, and the mixed solution was cooled to below 50°C, 1 part of a long-chain aliphatic compound, 0.2 parts of a phosphite antioxidant, and 0.2 parts of a liquid ultraviolet light absorber were added under stirring, and after reacting for 70 minutes, 0.02 parts of a modified imidazole accelerator were added to prepare a curing agent.
[0058] 1 part of epoxy resin mixture and 1.2 parts of curing agent were mixed evenly in proportion, the gel time was 200" at 160°C, cured at 70°C for 4h, then cured at 115°C for 2h, and finally cured at 150°C for 10h to obtain yellowing-resistant transparent flame-retardant epoxy resin cured product.
[0059] Example 7
[0060] A total of 8 parts of bisphenol A epoxy resin and hydrogenated epoxy resin and 2 parts of 3,4-epoxycyclohexylmethyl methacrylate are added into a reaction kettle and dispersed evenly to prepare an epoxy resin mixture for standby use; 8.6 parts of methyl nadic anhydride are heated to 80°C, 1.3 parts of DOPO flame retardant are added under stirring, and the mixture is stirred and kept warm until the DOPO flame retardant melts to form a mixed liquid, and the mixed liquid is cooled to below 50°C, 1 part of a long-chain aliphatic compound, 0.2 parts of 2,6-di-tert-butyl-p-cresol, and 0.2 parts of a liquid ultraviolet light absorber are added under stirring, and after reacting for 50 minutes, 0.02 parts of a BDMA accelerator are added to prepare a curing agent.
[0061] 1 part of epoxy resin mixture and 1.3 parts of curing agent were mixed uniformly in proportion, the gel time was 200" at 160°C, cured at 75°C for 4h, then cured at 100°C for 4h, and finally cured at 140°C for 10h to obtain a yellowing-resistant transparent flame-retardant epoxy resin cured product.
[0062] Example 8
[0063] A total of 8 parts of bisphenol A epoxy resin and bisphenol F epoxy resin, a total of 2 parts of 3,4-epoxycyclohexylcarboxylic acid-3',4'-epoxycyclohexyl methyl ester and bis((3,4-epoxycyclohexyl)methyl) adipate are added into a reaction kettle and dispersed evenly to prepare an epoxy resin mixture for standby use; a total of 8.6 parts of methyl nadic anhydride and methyl hexahydrophthalic anhydride are heated to 80°C, 1.3 parts of DOPO flame retardant are added under stirring, and the mixture is stirred and kept warm until the DOPO flame retardant melts to form a mixed solution, the mixed solution is cooled to below 50°C, 1 part of a long-chain aliphatic compound, 0.2 parts of a hindered phenol antioxidant, and 0.2 parts of a liquid ultraviolet light absorber are added under stirring, and after reacting for 55 minutes, 0.02 parts of a BDMA accelerator are added to prepare a curing agent.
[0064] 1 part of epoxy resin mixture and 1.4 parts of curing agent were mixed evenly in proportion, the gel time was 200" at 160°C, cured at 75°C for 4h, then cured at 100°C for 4h, and finally cured at 140°C for 10h to obtain a yellowing-resistant transparent flame-retardant epoxy resin cured product.
[0065] Example 9
[0066] A total of 8 parts of bisphenol A epoxy resin and bisphenol F epoxy resin, a total of 2 parts of 3,4-epoxycyclohexylcarboxylic acid-3',4'-epoxycyclohexyl methyl ester and bis((3,4-epoxycyclohexyl)methyl) adipate are added into a reaction kettle and dispersed evenly to prepare an epoxy resin mixture for standby use; a total of 8.6 parts of methyl nadic anhydride and methyl hexahydrophthalic anhydride are heated to 80°C, 1.3 parts of DOPO flame retardant are added under stirring, and the mixture is stirred and kept warm until the DOPO flame retardant melts to form a mixed solution, the mixed solution is cooled to below 50°C, 1 part of a long-chain aliphatic compound, 0.2 parts of a pentaerythritol diphosphite antioxidant, and 0.2 parts of a liquid ultraviolet light absorber are added under stirring, and after reacting for 60 minutes, a total of 0.02 parts of a modified imidazole accelerator and a modified phosphorus accelerator are added to prepare a curing agent.
[0067] 1 part of epoxy resin mixture and 0.7 part of curing agent were mixed evenly in proportion, the gel time was 200" at 160°C, cured at 75°C for 4h, then cured at 100°C for 4h, and finally cured at 140°C for 10h to obtain a yellowing-resistant transparent flame-retardant epoxy resin cured product.
[0068] Example 10
[0069] A total of 8 parts of bisphenol A epoxy resin and bisphenol F epoxy resin, a total of 2 parts of 3,4-epoxycyclohexylcarboxylic acid-3',4'-epoxycyclohexyl methyl ester and bis((3,4-epoxycyclohexyl)methyl) adipate are added into a reaction kettle and dispersed evenly to prepare an epoxy resin mixture for standby use; a total of 8.6 parts of methyl nadic anhydride and methyl hexahydrophthalic anhydride are heated to 80°C, 1.3 parts of DOPO flame retardant are added under stirring, and the mixture is stirred and kept warm until the DOPO flame retardant melts to form a mixed solution, the mixed solution is cooled to below 50°C, 1 part of a long-chain aliphatic compound, a total of 0.2 parts of hindered phenol antioxidants and pentaerythritol diphosphite antioxidants, and 0.2 parts of a liquid ultraviolet light absorber are added under stirring, and after reacting for 65 minutes, a total of 0.02 parts of a BDMA accelerator, a modified imidazole accelerator and a modified phosphorus accelerator are added to prepare a curing agent.
[0070] 1 part of epoxy resin mixture and 0.7 part of curing agent were mixed evenly in proportion, the gel time was 200" at 160°C, cured at 75°C for 4h, then cured at 100°C for 4h, and finally cured at 140°C for 10h to obtain a yellowing-resistant transparent flame-retardant epoxy resin cured product.
[0071] The performance test data of the cured epoxy resin adhesives prepared in Examples 1-6 of the present invention are shown in Table 1:
[0072] Table 1 Performance test data of epoxy resin adhesives prepared in Examples 1-6
[0073]
[0074]
[0075] As shown in Table 1, the epoxy resin adhesive prepared by the present invention has a bending strength of 90-110 MPa, an impact strength of 10-15 MPa, and a volume resistivity of more than 10 15 Ω·cm, light transmittance is 80%-90%, flame retardancy FV0 (6mm), baked at 150℃ for 10h, and the yellowing index of the resin sheet after curing is less than 8. The epoxy resin adhesive has excellent insulation performance, mechanical strength, high transparency and yellowing resistance. The adhesive of the present invention is a two-component solvent-free resin, which is cured at medium temperature. The product is transparent and colorless after curing, can withstand ultraviolet aging and heat aging without yellowing, has good flame retardant effect, and can effectively guarantee the mechanical properties and electrical properties of the material. It can be used as a potting material for electrical and electronic components, etc.; and the preparation method of the present invention is simple and easy, the material source is wide, the cost is low, and the use effect is good.
[0076] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A yellowing-resistant, transparent, flame-retardant epoxy resin adhesive, characterized in that: The invention comprises, by weight, 7 to 9 parts of epoxy resin, 1 to 3 parts of alicyclic epoxy resin, 7 to 9.5 parts of liquid acid anhydride, 1 to 2 parts of epoxy active toughening agent, 0.8 to 1.5 parts of DOPO flame retardant, 0.1 to 0.5 parts of antioxidant, 0.1 to 0.5 parts of ultraviolet light absorber and 0.01 to 1 parts of accelerator.
2. The yellowing-resistant transparent flame-retardant epoxy resin adhesive according to claim 1, characterized in that: The epoxy resin is one or more of bisphenol A epoxy resin, bisphenol F epoxy resin and hydrogenated epoxy resin.
3. The yellowing-resistant transparent flame-retardant epoxy resin adhesive according to claim 1, characterized in that: The alicyclic epoxy resin is one or more of 3,4-epoxycyclohexylcarboxylic acid-3',4'-epoxycyclohexyl methyl ester, bis((3,4-epoxycyclohexyl)methyl)adipate, poly[(2-oxiranyl)-1,2-cyclohexanediol]2-ethyl-2-(hydroxymethyl)-1,3-propylene glycol ether (3:1) and 3,4-epoxycyclohexyl methyl methacrylate.
4. The yellowing-resistant transparent flame-retardant epoxy resin adhesive according to claim 1, characterized in that: The liquid acid anhydride is one or more of methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride and methylnadic anhydride.
5. The yellowing-resistant transparent flame-retardant epoxy resin adhesive according to claim 1, characterized in that: The epoxy reactive toughening agent is one or more of a long-chain linear hydroxyl functional group polyether compound and a long-chain aliphatic compound.
6. The yellowing-resistant transparent flame-retardant epoxy resin adhesive according to claim 1, characterized in that: The DOPO flame retardant is 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide.
7. The yellowing-resistant transparent flame-retardant epoxy resin adhesive according to claim 1, characterized in that: The antioxidant is one or more of 2,6-di-tert-butyl-p-cresol, phosphite antioxidants, hindered phenol antioxidants and pentaerythritol diphosphite antioxidants.
8. The yellowing-resistant transparent flame-retardant epoxy resin adhesive according to claim 1, characterized in that: The ultraviolet light absorber is a liquid ultraviolet light absorber; the accelerator is one or more of BDMA, modified imidazoles, DBU salt and modified phosphorus accelerator.
9. The method for preparing a yellowing-resistant transparent flame-retardant epoxy resin adhesive according to claim 1, characterized in that: The following steps are involved: S1: mixing an epoxy resin and an alicyclic epoxy resin and dispersing them uniformly to obtain an epoxy resin mixture; S2: mixing liquid acid anhydride, epoxy active toughening agent, DOPO flame retardant, antioxidant, ultraviolet light absorber and accelerator together and dispersing them evenly to prepare epoxy resin curing agent; S3: The epoxy resin mixture and the epoxy resin curing agent are mixed in a mass ratio of 1:(0.7-1.3) to obtain a yellowing-resistant transparent flame-retardant epoxy resin adhesive.
10. The method for preparing a yellowing-resistant transparent flame-retardant epoxy resin adhesive according to claim 9, characterized in that: The S2 comprises the following steps: S21: heating the liquid acid anhydride to 60° C.-80° C., adding the DOPO flame retardant under stirring, and stirring at the same temperature until the DOPO flame retardant melts to form a mixed liquid; S22: Cool the mixed solution to below 50° C., add epoxy active toughening agent, antioxidant and ultraviolet light absorber under stirring, and add accelerator after reacting for 50 to 70 minutes to obtain epoxy resin curing agent.