Thermosensitive conductive adhesive and preparation method thereof

Through the combination of modified polyurethane and nano-copper wire, the problem of poor mechanical properties of conductive adhesives is solved, the conductivity, thermal sensitivity and flame retardant properties are improved, and the stability and safety of the battery are ensured.

CN118931455AInactive Publication Date: 2024-11-12SUZHOU LINGGUAN NEW ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411079650.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The mechanical properties of existing conductive adhesives are poor, resulting in battery bonding failure, electrolyte leakage and internal battery failure, affecting the stability and safety of the battery.

Method used

Using a combination of modified polyurethane, modified nanocopper wire, (3-acetamide propyl)trimethoxysilane and deionized water, a conjugated hydrogen bond six-membered ring is formed through the reaction of nanocopper wire surface graft and Schiff base. Structure, introducing phosphorus elements, forming an isolation protective layer and a crosslinking structure, improving conductivity, thermal sensitivity and flame retardant properties.

Benefits of technology

It significantly improves the conductivity, thermal sensitivity and flame retardant properties of the thermally sensitive conductive adhesive, enhances its stability and safety in high temperature environments, improves mechanical properties, and reduces battery failure rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004983336270000031
    Figure BDA0004983336270000031
  • Figure BDA0004983336270000032
    Figure BDA0004983336270000032
  • Figure BDA0004983336270000033
    Figure BDA0004983336270000033
Patent Text Reader

Abstract

The invention discloses a thermosensitive conductive adhesive and a preparation method thereof, and relates to the field of adhesives. When the thermosensitive conductive adhesive is prepared, a copper nano-wire sequentially reacts with 3-aminopropyltriethoxysilane and 2, 4-dihydroxybenzaldehyde to obtain a modified copper nano-wire; the preparation method comprises the following steps: reacting 1, 3, 5, 7-tetramethylcyclotetrasiloxane with 1, 3-bis (hydroxypropyl) tetramethyldisiloxane, and then reacting with dimethyl-vinyl phosphate to obtain functional double-terminal hydroxyl polysiloxane; the preparation method comprises the following steps: carrying out reaction on polyether glycol, p-phenylene diisocyanate and functional double-terminal hydroxyl polysiloxane to obtain modified polyurethane; and uniformly mixing the modified polyurethane, the modified nano copper wire, (3-acetamidopropyl) trimethoxysilane and deionized water to obtain the thermosensitive conductive adhesive. The thermosensitive conductive adhesive prepared by the preparation method disclosed by the invention has excellent heat sensitivity, conductivity, mechanical property and flame retardance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of adhesives, in particular to a heat-sensitive conductive adhesive and a preparation method thereof. Background Art

[0002] Conductive adhesive is a functional adhesive made by compounding conductive fillers with polymer matrix. The polymer matrix can provide excellent mechanical properties and viscosity, and conductive fillers with different surface morphologies and particle sizes can achieve the electrical and thermal conductivity of the adhesive. Compared with lead-tin welding, conductive adhesives have the advantages of high efficiency, low molding temperature, green environmental protection, and low cost. It is widely used in chip packaging, electromagnetic shielding protection, lithium battery connection and other fields. At present, many conductive adhesives on the market have poor mechanical properties. During use, the solution causes the battery bonding failure, causing electrolyte leakage and internal battery failure, affecting the stability and safety of the battery. Therefore, the present invention prepares a thermosensitive conductive adhesive with good mechanical properties. Summary of the invention

[0003] The object of the present invention is to provide a thermosensitive conductive adhesive and a preparation method thereof to solve the problems existing in the prior art.

[0004] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0005] A thermosensitive conductive adhesive is prepared by mixing modified polyurethane, modified nano copper wire, (3-acetamidopropyl)trimethoxysilane and deionized water.

[0006] As an optimization, the modified polyurethane is obtained by reacting polyether diol, p-phenylene diisocyanate and functional double-terminal hydroxyl polysiloxane.

[0007] As an optimization, the polyether diol model is 330HP, which comes from Shanghai Haoren International Trading Co., Ltd.

[0008] As an optimization, the functional double-terminal hydroxyl polysiloxane is obtained by reacting 1,3,5,7-tetramethylcyclotetrasiloxane with 1,3-bis(hydroxypropyl)tetramethyldisiloxane and then reacting with dimethyl-vinyl phosphate.

[0009] As an optimization, the modified nano copper wire is obtained by reacting the nano copper wire with 3-aminopropyltriethoxysilane and 2,4-dihydroxybenzaldehyde in sequence.

[0010] As an optimization, the nano copper wire model is BK2020061759, from Suzhou Kaifa New Materials Technology Co., Ltd.

[0011] A method for preparing a thermosensitive conductive adhesive comprises the following steps:

[0012] (1) mixing nano copper wire, 3-aminopropyltriethoxysilane and anhydrous ethanol in a mass ratio of 1: (0.04-0.06): (2-4), using a planetary centrifugal mixer, mixing at 1100-1300 r / min for 1-3 min, drying at 55-65° C. for 2-4 h, grinding and sieving 200-400 mesh to obtain pre-modified nano copper wire; mixing pre-modified nano copper wire, 2,4-dihydroxybenzaldehyde and anhydrous ethanol in a mass ratio of 1: (2-3): (24-26), refluxing at 75-85° C. and 200-300 rpm for 7-9 h, filtering, washing with deionized water for 3-5 times, and drying at 65-75° C. for 8-10 h to obtain modified nano copper wire;

[0013] (2) 1,3,5,7-tetramethylcyclotetrasiloxane and 1,3-bis(hydroxypropyl)tetramethyldisiloxane were mixed in a mass ratio of 1:(0.3-0.4), stirred at 65-75°C and 100-200 rpm for 10-20 min, added with trifluoromethylsulfonic acid (0.01-0.02 times the mass of 1,3,5,7-tetramethylcyclotetrasiloxane), continued stirring for 5-7 h, added with anhydrous sodium carbonate to adjust the pH to 6-7, filtered, and heated at 105-115°C and 0.1- Distill at 0.3MPa for 1-2h to obtain double-terminal hydroxyl hydrogenated silicone oil; mix double-terminal hydroxyl hydrogenated silicone oil, dimethyl-vinyl phosphate, chloroplatinic acid and toluene in a mass ratio of 1: (1.6-1.8): (0.01-0.02): (6-8), stir at 55-65°C and 100-200rpm for 11-13h under argon environment, heat to 70-80°C and continue stirring for 19-21h, cool naturally to room temperature, and distill under reduced pressure to obtain functional double-terminal hydroxyl polysiloxane;

[0014] (3) Mixing polyether diol and p-phenylene diisocyanate at a molar ratio of hydroxyl group to isocyanate group of 1:(2.4-2.6), stirring for 0.4-0.6 h at 70-80° C. and 400-500 rpm in a nitrogen atmosphere, adding dibutyltin dilaurate in an amount of 0.01-0.02 times the mass of the polyether diol, continuing stirring for 1-2 h, adding functional bi-terminal hydroxyl polysiloxane in an amount of 0.085-0.095 times the mass of the polyether diol, continuing stirring for 2-3 h, and naturally cooling to room temperature to obtain a modified polyurethane;

[0015] (4) The modified polyurethane, the modified nano copper wire, (3-acetamidopropyl)trimethoxysilane and deionized water are mixed in a mass ratio of 1:(3-4):(0.4-0.5):(1-2), stirred at 45-55° C. and 350-450 rpm for 1-3 h, and naturally cooled to room temperature to obtain a thermosensitive conductive adhesive.

[0016] As an optimization, the reaction equation of the pre-modified nano copper wire in step (1) is:

[0017]

[0018] As an optimization, the reaction equation of the modified nano copper wire in step (1) is:

[0019]

[0020] As an optimization, the reaction equation of the double-terminal hydroxyl hydrogenated silicone oil in step (2) is:

[0021]

[0022] As an optimization, the reaction equation of the functional double-terminal hydroxyl polysiloxane in step (2) is:

[0023]

[0024] As an optimization, the reaction equation of the modified polyurethane in step (3) is:

[0025]

[0026] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0027] When preparing the thermosensitive conductive adhesive, the present invention sequentially reacts nano copper wires with 3-aminopropyltriethoxysilane and 2,4-dihydroxybenzaldehyde to obtain modified nano copper wires; reacts 1,3,5,7-tetramethylcyclotetrasiloxane with 1,3-bis(hydroxypropyl)tetramethyldisiloxane and then reacts with dimethyl-vinyl phosphate to obtain functional double-terminal hydroxyl polysiloxane; reacts polyether diol, p-phenylene diisocyanate and functional double-terminal hydroxyl polysiloxane to obtain modified polyurethane; and mixes the modified polyurethane, modified nano copper wires, (3-acetamidopropyl)trimethoxysilane and deionized water to obtain the thermosensitive conductive adhesive.

[0028] Firstly, the nano copper wire is reacted with 3-aminopropyltriethoxysilane and 2,4-dihydroxybenzaldehyde in sequence to obtain modified nano copper wire; 1,3,5,7-tetramethylcyclotetrasiloxane and 1,3-bis(hydroxypropyl)tetramethyldisiloxane are reacted and then reacted with dimethyl-vinyl phosphate to obtain functional double-terminated hydroxyl polysiloxane; 3-aminopropyltriethoxysilane is grafted on the surface of the nano copper wire to improve the dispersibility of the nano copper wire and enhance the conductivity of the thermosensitive conductive adhesive; then a conjugated hydrogen bonded hexacyclic structure is formed through a Schiff base reaction. Under high temperature conditions, the increase in thermal motion within the molecule can cause the destruction and fracture of the conjugated structure, thereby improving the thermosensitivity of the thermosensitive conductive adhesive; dimethyl-vinyl phosphate is grafted through hydrosilylation to introduce phosphorus into the polymer matrix to capture free radicals in the combustion process and form an isolation protective layer to improve the flame retardant properties of the thermosensitive conductive adhesive.

[0029] Secondly, polyether diol, p-phenylene diisocyanate and functional double-terminated hydroxyl polysiloxane are reacted to obtain modified polyurethane; modified polyurethane, modified nano copper wire, (3-acetamidopropyl) trimethoxysilane and deionized water are mixed to obtain a thermosensitive conductive adhesive; a long silicon oxygen chain is introduced into the polyurethane main chain, and a silicon-carbon layer can be formed during the combustion process to isolate heat and oxygen, thereby improving the flame retardant properties of the thermosensitive conductive adhesive; the excess phenolic hydroxyl groups on the modified nano copper wire can form hydrogen bonds with the polyurethane main chain and (3-acetamidopropyl) trimethoxysilane to form crosslinks, thereby improving the mechanical properties of the thermosensitive conductive adhesive; at the same time, the thermal expansion coefficient of the polyurethane is much higher than that of the nano copper wire, and the polyurethane part expands in a high temperature environment, which expands the molecular distance, reduces the connection effect, and further improves the thermosensitivity of the thermosensitive conductive adhesive; (3-acetamidopropyl) trimethoxysilane is used to form a bonding layer between inorganic substrates to improve the adhesion of the thermosensitive conductive adhesive. DETAILED DESCRIPTION

[0030] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Example 1

[0032] A method for preparing a thermosensitive conductive adhesive, the method comprising the following steps:

[0033] (1) mixing nano copper wire, 3-aminopropyltriethoxysilane and anhydrous ethanol in a mass ratio of 1:0.04:2, using a planetary centrifugal mixer, mixing at 1100 r / min for 3 min, drying at 55° C. for 4 h, grinding and sieving 200 mesh to obtain pre-modified nano copper wire; mixing pre-modified nano copper wire, 2,4-dihydroxybenzaldehyde and anhydrous ethanol in a mass ratio of 1:2:24, refluxing at 75° C. and 200 rpm for 9 h, filtering, washing with deionized water 3 times, and drying at 65° C. for 10 h to obtain modified nano copper wire;

[0034] (2) 1,3,5,7-tetramethylcyclotetrasiloxane and 1,3-bis(hydroxypropyl)tetramethyldisiloxane were mixed in a mass ratio of 1:0.3, stirred at 65°C and 100 rpm for 20 min, trifluoromethylsulfonic acid (0.01 times the mass of 1,3,5,7-tetramethylcyclotetrasiloxane) was added, stirring was continued for 7 h, anhydrous sodium carbonate was added to adjust the pH to 6, and then filtered, distilled at 105°C and 0.1 MPa for 2 h to obtain a bihydroxy-terminated hydrogenated silicone oil; bihydroxy-terminated hydrogenated silicone oil, dimethyl-vinyl phosphate, chloroplatinic acid and toluene were mixed in a mass ratio of 1:1.6:0.01:6, stirred at 55°C and 100 rpm under argon environment for 13 h, heated to 70°C and stirred for 21 h, cooled naturally to room temperature, and distilled under reduced pressure to obtain a functional bihydroxy-terminated polysiloxane;

[0035] (3) polyether diol and p-phenylene diisocyanate were mixed at a molar ratio of hydroxyl group to isocyanate group of 1:2.4, stirred at 70°C and 400 rpm for 0.6 h in a nitrogen atmosphere, added with dibutyltin dilaurate at a mass of 0.01 times that of the polyether diol, and continued to stir for 2 h, added with functional bi-terminal hydroxyl polysiloxane at a mass of 0.085 times that of the polyether diol, and continued to stir for 3 h, and naturally cooled to room temperature to obtain a modified polyurethane;

[0036] (4) The modified polyurethane, the modified nano copper wire, (3-acetamidopropyl)trimethoxysilane and deionized water were mixed in a mass ratio of 1:3:0.4:1, stirred at 45° C. and 350 rpm for 3 h, and naturally cooled to room temperature to obtain a thermosensitive conductive adhesive.

[0037] Example 2

[0038] A method for preparing a thermosensitive conductive adhesive, the method comprising the following steps:

[0039] (1) mixing nano copper wire, 3-aminopropyltriethoxysilane and anhydrous ethanol in a mass ratio of 1:0.05:3, using a planetary centrifugal mixer, mixing at 1200r / min for 2min, drying at 60°C for 3h, grinding and sieving 300 mesh to obtain pre-modified nano copper wire; mixing pre-modified nano copper wire, 2,4-dihydroxybenzaldehyde and anhydrous ethanol in a mass ratio of 1:2.5:25, refluxing at 80°C and 250rpm for 8h, filtering, washing with deionized water 4 times, and drying at 70°C for 9h to obtain modified nano copper wire;

[0040] (2) 1,3,5,7-tetramethylcyclotetrasiloxane and 1,3-bis(hydroxypropyl)tetramethyldisiloxane were mixed in a mass ratio of 1:0.35, stirred at 70°C and 150 rpm for 15 min, trifluoromethylsulfonic acid (0.015 times the mass of 1,3,5,7-tetramethylcyclotetrasiloxane) was added, stirring was continued for 6 h, anhydrous sodium carbonate was added to adjust the pH to 6.5, and then filtered, distilled at 110°C and 0.2 MPa for 1.5 h to obtain a bihydroxy-terminated hydrogenated silicone oil; bihydroxy-terminated hydrogenated silicone oil, dimethyl-vinyl phosphate, chloroplatinic acid and toluene were mixed in a mass ratio of 1:1.7:0.05:7, stirred at 60°C and 150 rpm under argon environment for 12 h, heated to 75°C and stirred for 20 h, cooled naturally to room temperature, and distilled under reduced pressure to obtain a functional bihydroxy-terminated polysiloxane;

[0041] (3) polyether diol and p-phenylene diisocyanate were mixed at a molar ratio of hydroxyl group to isocyanate group of 1:2.5, stirred at 75°C and 450 rpm for 0.5 h in a nitrogen atmosphere, added with dibutyltin dilaurate in an amount of 0.015 times the mass of the polyether diol, and continued to stir for 1.5 h, added with functional bi-terminal hydroxyl polysiloxane in an amount of 0.09 times the mass of the polyether diol, and continued to stir for 2.5 h, and naturally cooled to room temperature to obtain a modified polyurethane;

[0042] (4) The modified polyurethane, the modified nano copper wire, (3-acetamidopropyl)trimethoxysilane and deionized water were mixed in a mass ratio of 1:3.5:0.45:1.5, stirred at 50° C. and 400 rpm for 2 h, and naturally cooled to room temperature to obtain a thermosensitive conductive adhesive.

[0043] Example 3

[0044] A method for preparing a thermosensitive conductive adhesive, the method comprising the following steps:

[0045] (1) mixing nano copper wire, 3-aminopropyltriethoxysilane and anhydrous ethanol in a mass ratio of 1:0.06:4, mixing at 1300 r / min for 1 min using a planetary centrifugal mixer, drying at 65° C. for 2 h, grinding and sieving through 400 mesh to obtain pre-modified nano copper wire; mixing pre-modified nano copper wire, 2,4-dihydroxybenzaldehyde and anhydrous ethanol in a mass ratio of 1:3:26, refluxing at 85° C. and 300 rpm for 7 h, filtering, washing with deionized water for 5 times, and drying at 75° C. for 8 h to obtain modified nano copper wire;

[0046] (2) 1,3,5,7-tetramethylcyclotetrasiloxane and 1,3-bis(hydroxypropyl)tetramethyldisiloxane were mixed in a mass ratio of 1:0.4, stirred at 75°C and 200 rpm for 10 min, trifluoromethylsulfonic acid was added in an amount of 0.02 times the mass of 1,3,5,7-tetramethylcyclotetrasiloxane, and stirring was continued for 5 h, anhydrous sodium carbonate was added to adjust the pH to 7, and then filtered, and distilled at 115°C and 0.3 MPa for 1 h to obtain a bihydroxy-terminated hydrogenated silicone oil; bihydroxy-terminated hydrogenated silicone oil, dimethyl-vinyl phosphate, chloroplatinic acid and toluene were mixed in a mass ratio of 1:1.8:0.02:8, stirred at 65°C and 200 rpm under argon environment for 11 h, heated to 80°C and stirred for 19 h, cooled naturally to room temperature, and distilled under reduced pressure to obtain a functional bihydroxy-terminated polysiloxane;

[0047] (3) polyether diol and p-phenylene diisocyanate were mixed at a molar ratio of hydroxyl group to isocyanate group of 1:2.6, stirred at 80°C and 500 rpm for 0.4 h in a nitrogen atmosphere, added with dibutyltin dilaurate in an amount of 0.02 times the mass of the polyether diol, continued to stir for 1 h, added with functional bi-terminal hydroxyl polysiloxane in an amount of 0.095 times the mass of the polyether diol, continued to stir for 2 h, and naturally cooled to room temperature to obtain a modified polyurethane;

[0048] (4) The modified polyurethane, the modified nano copper wire, (3-acetamidopropyl)trimethoxysilane and deionized water were mixed in a mass ratio of 1:4:0.5:2, stirred at 55° C. and 450 rpm for 1 h, and naturally cooled to room temperature to obtain a thermosensitive conductive adhesive.

[0049] Comparative Example 1

[0050] A method for preparing a thermosensitive conductive adhesive, the method comprising the following steps:

[0051] (1) 1,3,5,7-tetramethylcyclotetrasiloxane and 1,3-bis(hydroxypropyl)tetramethyldisiloxane were mixed in a mass ratio of 1:0.35, stirred at 70°C and 150 rpm for 15 min, trifluoromethylsulfonic acid was added in an amount of 0.015 times the mass of 1,3,5,7-tetramethylcyclotetrasiloxane, and stirring was continued for 6 h, anhydrous sodium carbonate was added to adjust the pH to 6.5, and then filtered, and distilled at 110°C and 0.2 MPa for 1.5 h to obtain a bihydroxy-terminated hydrogenated silicone oil; bihydroxy-terminated hydrogenated silicone oil, dimethyl-vinyl phosphate, chloroplatinic acid and toluene were mixed in a mass ratio of 1:1.7:0.05:7, stirred at 60°C and 150 rpm under an argon environment for 12 h, heated to 75°C and stirred for 20 h, cooled naturally to room temperature, and distilled under reduced pressure to obtain a functional bihydroxy-terminated polysiloxane;

[0052] (2) polyether diol and p-phenylene diisocyanate were mixed at a molar ratio of hydroxyl group to isocyanate group of 1:2.5, stirred at 75°C and 450 rpm for 0.5 h in a nitrogen atmosphere, added with dibutyltin dilaurate in an amount of 0.015 times the mass of the polyether diol, and continued to stir for 1.5 h, added with functional bi-terminal hydroxyl polysiloxane in an amount of 0.09 times the mass of the polyether diol, and continued to stir for 2.5 h, and naturally cooled to room temperature to obtain a modified polyurethane;

[0053] (3) The modified polyurethane, the modified nano copper wire, (3-acetamidopropyl)trimethoxysilane and deionized water were mixed in a mass ratio of 1:3.5:0.45:1.5, stirred at 50° C. and 400 rpm for 2 h, and naturally cooled to room temperature to obtain a thermosensitive conductive adhesive.

[0054] Comparative Example 2

[0055] A method for preparing a thermosensitive conductive adhesive, the method comprising the following steps:

[0056] (1) mixing nano copper wire, 3-aminopropyltriethoxysilane and anhydrous ethanol in a mass ratio of 1:0.05:3, using a planetary centrifugal mixer, mixing at 1200r / min for 2min, drying at 60°C for 3h, grinding and sieving 300 mesh to obtain pre-modified nano copper wire; mixing pre-modified nano copper wire, 2,4-dihydroxybenzaldehyde and anhydrous ethanol in a mass ratio of 1:2.5:25, refluxing at 80°C and 250rpm for 8h, filtering, washing with deionized water 4 times, and drying at 70°C for 9h to obtain modified nano copper wire;

[0057] (2) 1,3,5,7-tetramethylcyclotetrasiloxane and 1,3-bis(hydroxypropyl)tetramethyldisiloxane were mixed at a mass ratio of 1:0.35, stirred at 70°C and 150 rpm for 15 min, trifluoromethylsulfonic acid (0.015 times the mass of 1,3,5,7-tetramethylcyclotetrasiloxane) was added, and stirring was continued for 6 h. Anhydrous sodium carbonate was added to adjust the pH to 6.5, and then filtered, and distilled at 110°C and 0.2 MPa for 1.5 h to obtain a double-terminal hydroxyl hydrogenated silicone oil;

[0058] (3) polyether diol and p-phenylene diisocyanate were mixed at a molar ratio of hydroxyl group to isocyanate group of 1:2.5, stirred at 75°C and 450 rpm for 0.5 h in a nitrogen atmosphere, added with dibutyltin dilaurate in an amount of 0.015 times the mass of the polyether diol, and continued to stir for 1.5 h, added with dibutyltin dilaurate in an amount of 0.09 times the mass of the polyether diol, and continued to stir for 2.5 h, and naturally cooled to room temperature to obtain a modified polyurethane;

[0059] (4) The modified polyurethane, the modified nano copper wire, (3-acetamidopropyl)trimethoxysilane and deionized water were mixed in a mass ratio of 1:3.5:0.45:1.5, stirred at 50° C. and 400 rpm for 2 h, and naturally cooled to room temperature to obtain a thermosensitive conductive adhesive.

[0060] Comparative Example 3

[0061] A method for preparing a thermosensitive conductive adhesive, the method comprising the following steps:

[0062] (1) mixing nano copper wire, 3-aminopropyltriethoxysilane and anhydrous ethanol in a mass ratio of 1:0.05:3, using a planetary centrifugal mixer, mixing at 1200r / min for 2min, drying at 60°C for 3h, grinding and sieving 300 mesh to obtain pre-modified nano copper wire; mixing pre-modified nano copper wire, 2,4-dihydroxybenzaldehyde and anhydrous ethanol in a mass ratio of 1:2.5:25, refluxing at 80°C and 250rpm for 8h, filtering, washing with deionized water 4 times, and drying at 70°C for 9h to obtain modified nano copper wire;

[0063] (2) polyether diol and p-phenylene diisocyanate were mixed at a molar ratio of hydroxyl group to isocyanate group of 1:2.5, stirred at 75° C. and 450 rpm for 0.5 h in a nitrogen atmosphere, and dibutyltin dilaurate (0.015 times the mass of the polyether diol) was added, and stirring was continued for 1.5 h, and the mixture was naturally cooled to room temperature to obtain a polyurethane;

[0064] (3) The polyurethane, modified nano copper wire, (3-acetamidopropyl)trimethoxysilane and deionized water were mixed in a mass ratio of 1:3.5:0.45:1.5, stirred at 50° C. and 400 rpm for 2 h, and naturally cooled to room temperature to obtain a thermosensitive conductive adhesive.

[0065] Test Case

[0066] The thermosensitive conductive adhesive obtained in each example and the comparative example were coated on a polytetrafluoroethylene film to a thickness of 3 mm, and cured at 60° C. for 24 hours to obtain a thermosensitive conductive adhesive film.

[0067] 1. Thermal conductivity

[0068] Test method: The volume resistivity of the thermosensitive conductive adhesive film obtained in each example and the comparative example was tested at 30°C and 140°C respectively using a HPS2661 four-probe resistivity tester in accordance with GB / T31838.

[0069] 2. Mechanical properties

[0070] Test method: The thermosensitive conductive adhesive films obtained in each example and the comparative example were tested for tensile strength σ0 at a rate of 200 mm / min according to GB / T528.

[0071] 3. Flame retardancy

[0072] Test method: The thermosensitive conductive adhesive films obtained in each example and the comparative example were cut into samples of 100 mm×6 mm in size, and the limiting oxygen index was tested according to GB / T2406.

[0073] Table 1 below shows the analysis results of the thermal sensitivity, electrical conductivity, mechanical properties and flame retardancy of the thermally conductive adhesives of Examples 1 to 3 of the present invention and Comparative Examples 1 to 3.

[0074] Table 1

[0075]

[0076]

[0077] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 3 in Table 1, it can be found that the thermosensitive conductive adhesive prepared in the present invention has good thermosensitivity, conductivity, mechanical properties and flame retardancy.

[0078] By comparison, compared with Example 1, Examples 1, 2, and 3, the volume resistivity at 30°C is lower and the volume resistivity at 140°C and the tensile strength are higher, which indicates that 3-aminopropyltriethoxysilane is grafted on the surface of nano-copper wires to improve the dispersibility of nano-copper wires and enhance the conductivity of the thermosensitive conductive adhesive; the thermal expansion coefficient of polyurethane is much higher than that of nano-copper wires. In a high temperature environment, the polyurethane part expands, the molecular distance is enlarged, the connection effect is reduced, and the thermosensitivity of the thermosensitive conductive adhesive is improved; at the same time, a conjugated hydrogen bond hexacyclic structure is formed through the Schiff base reaction. In a high temperature environment, the increase in thermal motion inside the molecule can cause the destruction and fracture of the conjugated structure, further improving the thermosensitivity of the thermosensitive conductive adhesive; the excess phenolic hydroxyl groups on the modified nano-copper wires can form hydrogen bonds with the polyurethane main chain and (3-acetamidopropyl)trimethoxysilane to form crosslinks, thereby improving the mechanical properties of the thermosensitive conductive adhesive.

[0079] By comparison, the limiting oxygen index of Examples 1, 2, and 3 is lower than that of Comparative Example 2, which indicates that phosphorus is introduced into the polymer matrix through the hydrosilylation grafting of dimethyl-vinyl phosphate to capture free radicals in the combustion process and form an isolation protective layer, thereby improving the flame retardant properties of the thermosensitive conductive adhesive.

[0080] By comparison, the limiting oxygen index of Examples 1, 2, and 3 is lower than that of Comparative Example 3, indicating that the introduction of long silicon-oxygen chains on the polyurethane main chain can form a silicon-carbon layer during the combustion process, isolate heat and oxygen, and improve the flame retardant properties of the thermosensitive conductive adhesive.

[0081] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A heat-sensitive conductive adhesive, It is characterized in that The thermosensitive conductive adhesive is obtained by mixing modified polyurethane, modified nano copper wire, (3-acetamidopropyl)trimethoxysilane and deionized water; The modified polyurethane is obtained by reacting polyether diol, p-phenylene diisocyanate and functional double-terminal hydroxyl polysiloxane; The functional double-terminal hydroxyl polysiloxane is obtained by reacting 1,3,5,7-tetramethylcyclotetrasiloxane and 1,3-bis(hydroxypropyl)tetramethyldisiloxane, and then reacting with dimethyl-vinyl phosphate; The modified nano copper wire is obtained by sequentially reacting the nano copper wire with 3-aminopropyltriethoxysilane and 2,4-dihydroxybenzaldehyde.

2. A method for preparing a thermosensitive conductive adhesive, It is characterized in that The method comprises the following preparation steps: (1) mixing nano copper wire, 3-aminopropyltriethoxysilane and anhydrous ethanol in a mass ratio of 1: (0.04-0.06): (2-4), using a planetary centrifugal mixer, mixing at 1100-1300 r / min for 1-3 min, drying at 55-65° C. for 2-4 h, grinding and sieving 200-400 mesh to obtain pre-modified nano copper wire; mixing pre-modified nano copper wire, 2,4-dihydroxybenzaldehyde and anhydrous ethanol in a mass ratio of 1: (2-3): (24-26), refluxing at 75-85° C. and 200-300 rpm for 7-9 h, filtering, washing with deionized water for 3-5 times, and drying at 65-75° C. for 8-10 h to obtain modified nano copper wire; (2) 1,3,5,7-tetramethylcyclotetrasiloxane and 1,3-bis(hydroxypropyl)tetramethyldisiloxane were mixed in a mass ratio of 1:(0.3-0.4), stirred at 65-75°C and 100-200 rpm for 10-20 min, added with trifluoromethylsulfonic acid (0.01-0.02 times the mass of 1,3,5,7-tetramethylcyclotetrasiloxane), continued stirring for 5-7 h, added with anhydrous sodium carbonate to adjust the pH to 6-7, filtered, and heated at 105-115°C and 0.1- Distill at 0.3MPa for 1-2h to obtain double-terminal hydroxyl hydrogenated silicone oil; mix double-terminal hydroxyl hydrogenated silicone oil, dimethyl-vinyl phosphate, chloroplatinic acid and toluene in a mass ratio of 1: (1.6-1.8): (0.01-0.02): (6-8), stir at 55-65°C and 100-200rpm for 11-13h under argon environment, heat to 70-80°C and continue stirring for 19-21h, cool naturally to room temperature, and distill under reduced pressure to obtain functional double-terminal hydroxyl polysiloxane; (3) Mixing polyether diol and p-phenylene diisocyanate at a molar ratio of hydroxyl group to isocyanate group of 1:(2.4-2.6), stirring for 0.4-0.6 h at 70-80° C. and 400-500 rpm in a nitrogen atmosphere, adding dibutyltin dilaurate in an amount of 0.01-0.02 times the mass of the polyether diol, continuing stirring for 1-2 h, adding functional bi-terminal hydroxyl polysiloxane in an amount of 0.085-0.095 times the mass of the polyether diol, continuing stirring for 2-3 h, and naturally cooling to room temperature to obtain a modified polyurethane; (4) The modified polyurethane, the modified nano copper wire, (3-acetamidopropyl)trimethoxysilane and deionized water are mixed in a mass ratio of 1:(3-4):(0.4-0.5):(1-2), stirred at 45-55° C. and 350-450 rpm for 1-3 h, and naturally cooled to room temperature to obtain a thermosensitive conductive adhesive.

3. A method for preparing a thermosensitive conductive adhesive according to claim 2, It is characterized in that The reaction equation of the pre-modified nano copper wire in step (1) is:

4. A method for preparing a thermosensitive conductive adhesive according to claim 2, It is characterized in that The reaction equation of the modified nano copper wire in step (1) is:

5. A method for preparing a thermosensitive conductive adhesive according to claim 2, It is characterized in that The reaction equation of the double-terminal hydroxyl hydrogenated silicone oil in step (2) is:

6. A method for preparing a thermosensitive conductive adhesive according to claim 2, It is characterized in that The reaction equation of the functional double-terminal hydroxyl polysiloxane in step (2) is:

7. A method for preparing a thermosensitive conductive adhesive according to claim 2, It is characterized in that The reaction equation of the modified polyurethane in step (3) is:

Citation Information

Cited By

  • Method for producing high-activity and high-melting-point isocyanate prepolymer and product thereof in small batch

    CN120535722A