Moisture curing reaction type polyurethane hot melt adhesive and preparation method thereof

By optimizing the ratio of components such as polyether polyol, polyester polyol, and isocyanate and strictly controlling the moisture content, a moisture-curing reactive polyurethane hot melt adhesive suitable for automatic edge sealing of furniture was prepared. This solved the problems of high cost or unsuitable opening time, and achieved efficient and low-cost edge sealing results.

CN118931457APending Publication Date: 2024-11-12LANGFANG HUAYU INNOVATION TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411226407.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing moisture-curing reactive polyurethane hot melt adhesives have problems such as high cost or unsuitable opening time in furniture edge banding operations, making it difficult to meet the needs of automated and high-efficiency operations.

Method used

Using polyether polyol, polyester polyol, isocyanate, and tackifying resin in specific proportions as main materials, and adding catalysts, chain extenders, and coupling agents, a moisture-curing reactive polyurethane hot melt adhesive with a suitable open time is prepared by strictly controlling the water content of the polyol composition.

Benefits of technology

A moisture-curing reactive polyurethane hot melt adhesive with low cost and moderate open time was prepared to meet the requirements of automatic edge sealing operations for furniture and has high peel strength after curing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005024703310000021
    Figure BDA0005024703310000021
  • Figure BDA0005024703310000071
    Figure BDA0005024703310000071
  • Figure FDA0005024703300000011
    Figure FDA0005024703300000011
Patent Text Reader

Abstract

According to the moisture curing reaction type polyurethane hot melt adhesive and the preparation method, polyether polyol, polyester polyol, isocyanate and tackifying resin are used as main materials, a catalyst, a chain extender and a coupling agent are added, and the moisture curing reaction type polyurethane hot melt adhesive (PUR) which is low in cost and moderate in opening time is prepared; the adhesive provided by the invention is suitable for spraying or roller operation, has high peel strength after curing, can completely meet the requirements of automatic edge sealing operation of furniture, and overcomes the problems of high cost or improper opening time in the prior art.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of adhesives, and in particular to a moisture-curing reactive polyurethane hot melt adhesive for automatic edge sealing of furniture. Background Art

[0002] At present, the furniture edge banding adhesives used in the market include solvent-based adhesives, water-based adhesives and EVA hot melt adhesives. Among them, solvent-based adhesives have the advantages of strong bonding and good coating properties, but the solvents contained in them are easy to volatilize toxic gases during the preparation of adhesives and the subsequent use process, which not only pollutes the environment but also harms the health of operators; water-based adhesives are adhesives that use water as a dispersion medium. In addition to the excellent properties of solvent-based adhesives, they also have the advantages of being non-flammable and non-explosive, non-toxic, and non-polluting the environment. However, due to the large surface tension of water, the surface spreading of water-based adhesives during film formation is poor, the drying time is long, and the film-forming and substrate composite is poor, resulting in reduced mechanical properties; while EVA hot melt adhesives have the advantages of fast bonding speed, non-toxicity, non-flammability, and a wide range of applications, but poor rigidity after curing, low softening point, and poor heat resistance, which limits its wide range of applications. In order to overcome the above problems, moisture-curing reactive polyurethane hot melt adhesive (PUR) is a type of adhesive that is currently being rapidly developed and applied. It has excellent properties such as environmental protection, heat resistance, cold resistance, water resistance, and solvent resistance. Moreover, due to its reaction curing to form a cross-linked structure, the bonding strength is greatly improved, and it is currently a hot topic in the research of environmentally friendly adhesives.

[0003] Although reactive polyurethane hot melt adhesive has many advantages, its price is higher than that of ordinary adhesives, resulting in high cost of use, and the open time is generally more than 3 minutes to obtain a strong initial bonding strength. However, the current furniture edge banding is developing towards automation and high efficiency, and the hot melt adhesive needs to have a shorter open time. Patent 202110723056.X discloses a reactive moisture-curing polyurethane hot melt adhesive for furniture edge banding and a preparation method thereof. After prepolymerization of non-crystalline polyester, polycarbonate polyol and high molecular weight copolyester, copolymerization under the action of a chain extender obtains a high molecular weight polymer, shortening the PUR open time to less than 20 seconds. Although the open time is shorter, for certain working environments such as large items, the open time is too short, and the adhesive cures too quickly after coating, which is not conducive to the furniture edge banding operation. In actual production, the cost of hot melt adhesive is also one of the important factors in product competitiveness. Patent 202110723056.X has a higher cost due to the addition of more EVA and high molecular weight copolyester. Therefore, how to design an adhesive with an open time between 25 and 40 seconds and low cost while meeting the needs of efficient edge banding operations is still an important research and optimization direction for current reactive polyurethane hot melt adhesives. Summary of the invention

[0004] In view of the above problems, the present application aims to provide a moisture-curing reactive polyurethane hot melt adhesive, which not only maintains excellent properties such as environmental protection, heat resistance, cold resistance, and water resistance, but also has low material selection requirements, a wide range of material sources, a low production cost, and a moderate open time, and can meet the operational requirements of automatic edge sealing of furniture.

[0005] In a first aspect, the present application provides a moisture-curing reactive polyurethane hot melt adhesive, the hot melt adhesive comprising the following components in parts by weight:

[0006]

[0007] According to the technical solution provided in the embodiment of the present application, the hydroxyl value of the polyether polyol is 30-500 mgKOH / g, and the functionality is 3.0; the hydroxyl value of the polyester polyol is 30-500 mgKOH / g, and the functionality is 3.0.

[0008] According to the technical solution provided in the embodiment of the present application, the polyether polyol includes one or two of 310, 330N or 3050 of Langfang Quanzhen Chemical Development Co., Ltd.

[0009] According to the technical solution provided in the embodiment of the present application, the polyester polyol includes one or more of PL5601, PL1201 or white polyester produced by Qingdao Ruinuo Chemical Co., Ltd.

[0010] According to the technical solution provided in the embodiment of the present application, the isocyanate includes diisocyanate (NCO), preferably one or more of diphenylmethane diisocyanate (MDI), toluene diisocyanate (TDI), hexamethylene diisocyanate (HDI) or isophorone diisocyanate (IPDI).

[0011] According to the technical solution provided in the embodiment of the present application, the tackifying resin includes one or both of rosin resin and terpene resin.

[0012] According to the technical solution provided in the embodiment of the present application, the catalyst includes one or more of bismorpholine diethyl ether, triethylenediamine or dibutyltin dilaurate.

[0013] According to the technical solution provided in the embodiment of the present application, the chain extender includes 1,4-butanediol, ethylene glycol or trimethylolpropane; the coupling agent is a silane coupling agent, preferably KH550 from Langfang Quanzhen Chemical Development Co., Ltd.

[0014] In a second aspect, the present application also provides a method for preparing a moisture-curing reactive polyurethane hot melt adhesive, the preparation method comprising the following steps:

[0015] Step 1: Mixing polyether polyol and polyester polyol, stirring, heating, and vacuum dehydrating to obtain a polyol composition, wherein the stirring speed is 60 to 80 r / min, the heating temperature is 100 to 120° C., and the vacuum degree is -0.8 to -1.0 MPa;

[0016] Step 2: mixing the polyol composition and the isocyanate to obtain a prepolymer, wherein the temperature of the polyol composition needs to be reduced to 50-90° C., and then adding the isocyanate to obtain a prepolymer after reaction;

[0017] Step 3: lowering the temperature of the prepolymer to ≤50° C., adding the tackifying resin, the catalyst, the chain extender, and the coupling agent to the prepolymer, and mixing them evenly to obtain the hot melt adhesive.

[0018] According to the technical solution provided in the examples of the present application, the water content of the polyol composition is less than 0.015%.

[0019] Specifically, since water can react with isocyanate and consume the content of isocyanate, thus affecting the effect of adding isocyanate and ultimately affecting the quality of the finished product of polyurethane hot melt adhesive, this application needs to strictly control the water content in the polyol composition through the process, and reduce the water content of the polyol composition to below 0.015%, so as to accurately control the amount of isocyanate added in the later stage, ensure the quality of hot melt adhesive, and provide an accurate judgment basis. Moreover, a lower water content is also conducive to extending the storage life of polyurethane hot melt adhesive.

[0020] In summary, the present application discloses a moisture-curing reactive polyurethane hot melt adhesive. The beneficial effect produced based on the above scheme is that the present application uses polyether polyol, polyester polyol, isocyanate and tackifying resin as main materials, adds catalyst, chain extender and coupling agent, and prepares a low-cost, moderately open time moisture-curing reactive polyurethane hot melt adhesive (PUR). The open time is 25 to 35 seconds, which is more suitable for large-scale furniture spraying or roller operation, and the peel strength after curing is relatively high, which can fully meet the operation requirements of automatic edge sealing of furniture, and overcomes the problems of high cost or inappropriate open time in the prior art. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] none. DETAILED DESCRIPTION

[0022] The present application is further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the relevant invention, rather than to limit the invention.

[0023] Example 1

[0024] A moisture-curing reactive polyurethane hot melt adhesive is prepared by weighing, by weight, 25 parts of polyether polyol, 34 parts of polyester polyol, 23 parts of isocyanate, 16 parts of tackifying resin, 0.2 parts of catalyst, 1.0 parts of chain extender and 0.8 parts of coupling agent. The hydroxyl value of the polyether polyol and the polyester polyol is 30-500 mgKOH / g, and the functionality is 3.0.

[0025] Among them, the polyether polyol is 310 from Langfang Quanzhen Chemical Development Co., Ltd., the polyester polyol is white polyester, the isocyanate is MDI (diphenylmethane diisocyanate), the tackifying resin is rosin resin, the chain extender is 1,4-butanediol, the coupling agent is KH550 from Langfang Quanzhen Chemical Development Co., Ltd., and the catalyst is bismorpholine diethyl ether.

[0026] The preparation process of hot melt adhesive includes the following steps:

[0027] Step 1: Pour polyether polyol and polyester polyol into a container, heat and stir, and when the temperature reaches 100° C., start vacuuming and dehydration. When the water content of the polyol composition is 0.01%, stop vacuuming to obtain a polyol composition, wherein the rotation speed of the stirring process is 80 r / min and the vacuum degree is -1.0 MPa;

[0028] Step 2: lowering the temperature of the polyol composition to 90° C., then pouring isocyanate into a container and mixing it with the polyol composition to obtain a prepolymer after reaction;

[0029] Step 3: Cool the prepolymer to 30° C., then add a tackifying resin, a chain extender, a coupling agent, and a catalyst to the prepolymer, and mix them evenly to obtain a polyurethane hot melt adhesive.

[0030] Example 2

[0031] A moisture-curing reactive polyurethane hot melt adhesive is prepared by weighing, by weight, 21 parts of polyether polyol, 38 parts of polyester polyol, 25 parts of isocyanate, 15 parts of tackifying resin, 0.1 parts of catalyst, 0.6 parts of chain extender and 0.3 parts of coupling agent. The hydroxyl value of the polyether polyol and the polyester polyol is 30-500 mgKOH / g, and the functionality is 3.0.

[0032] Among them, the polyether polyol is 3050 from Langfang Quanzhen Chemical Development Co., Ltd., the polyester polyol is PL5601 from Qingdao Ruinuo Chemical Co., Ltd., the isocyanate is TDI (toluene diisocyanate), the tackifying resin is terpene resin, the chain extender is ethylene glycol, the coupling agent is KH550 from Langfang Quanzhen Chemical Development Co., Ltd., and the catalyst is triethylenediamine.

[0033] The preparation process of hot melt adhesive includes the following steps:

[0034] Step 1: Pour polyether polyol and polyester polyol into a container, heat and stir, and when the temperature reaches 120° C., start vacuuming and dehydration. When the water content of the polyol composition is 0.012%, stop vacuuming to obtain a polyol composition, wherein the rotation speed of the stirring process is 60 r / min and the vacuum degree is -0.8 MPa;

[0035] Step 2: lowering the temperature of the polyol composition to 50° C., then pouring isocyanate into a container and mixing it with the polyol composition to obtain a prepolymer after reaction;

[0036] Step 3: Cool the prepolymer to 20° C., then add a tackifying resin, a chain extender, a coupling agent, and a catalyst to the prepolymer, and mix them evenly to obtain a polyurethane hot melt adhesive.

[0037] Example 3

[0038] A moisture-curing reactive polyurethane hot melt adhesive is provided. The invention discloses a moisture-curing reactive polyurethane hot melt adhesive. The adhesive comprises 22 parts of polyether polyol, 33 parts of polyester polyol, 27 parts of isocyanate, 17 parts of tackifying resin, 0.2 parts of catalyst, 0.5 parts of chain extender and 0.3 parts of coupling agent, and the hydroxyl values ​​of the polyether polyol and the polyester polyol are 30-500 mgKOH / g.

[0039] Among them, the polyether polyol is a mixture of 330N and 3050 produced by Langfang Quanzhen Chemical Development Co., Ltd., the functionality of 330N is 3.0, and the functionality of 3050 is 3.0. The polyester polyol is PL1201 produced by Qingdao Ruinuo Chemical Co., Ltd., with a functionality of 3.0. The isocyanate is a mixture of HDI (hexamethylene diisocyanate) and IPDI (isophorone diisocyanate). The tackifying resin is terpene resin, the chain extender is trimethylolpropane, the coupling agent is KH550 produced by Langfang Quanzhen Chemical Development Co., Ltd., and the catalyst is a mixture of dibutyltin dilaurate and triethylenediamine.

[0040] The preparation process of hot melt adhesive includes the following steps:

[0041] Step 1: Pour polyether polyol and polyester polyol into a container, heat and stir, and when the temperature reaches 110° C., start vacuuming and dehydration. When the water content of the polyol composition is 0.01%, stop vacuuming to obtain a polyol composition, wherein the rotation speed of the stirring process is 65 r / min and the vacuum degree is -0.9 MPa;

[0042] Step 2: lowering the temperature of the polyol composition to 80° C., then pouring isocyanate into a container and mixing it with the polyol composition to obtain a prepolymer after reaction;

[0043] Step 3: Cool the prepolymer to 50° C., then add a tackifying resin, a chain extender, a coupling agent, and a catalyst to the prepolymer, and mix them evenly to obtain a polyurethane hot melt adhesive.

[0044] Comparative Example 1

[0045] Compared with Example 3, the only difference is that

[0046] A moisture-curing reactive polyurethane hot melt adhesive comprises 30 parts of polyether polyol, 30 parts of polyester polyol, 28 parts of isocyanate and 11 parts of tackifying resin, measured in parts by weight.

[0047] Comparative Example 2

[0048] Compared with Example 3, the only difference is that

[0049] A moisture-curing reactive polyurethane hot melt adhesive comprises 18 parts of polyether polyol, 40 parts of polyester polyol, 29 parts of isocyanate and 12 parts of tackifying resin, measured in parts by weight.

[0050] Comparative Example 3

[0051] Compared with Example 3, the only difference is that

[0052] A moisture-curing reactive polyurethane hot melt adhesive comprises 40 parts of polyether polyol, 18 parts of polyester polyol, 28 parts of isocyanate and 13 parts of tackifying resin, measured in parts by weight.

[0053] Comparative Example 4

[0054] Compared with Example 1, the only difference is that

[0055] The polyether polyol was 2020 from Langfang Quanzhen Chemical Development Co., Ltd., and its functionality was 2.0.

[0056] Comparative Example 5

[0057] Compared with Example 1, the only difference is that

[0058] The polyester polyol is an amorphous polyester from Suzhou Hanhai New Materials Co., Ltd., and its functionality is 2.0.

[0059] Comparative Example 6

[0060] Compared with Example 1, the only difference is that

[0061] The dehydration pressure was -0.4 MPa; after dehydration, the water content of the polyol composition was 0.07%.

[0062] Comparative Example 7

[0063] Compared with Example 1, the only difference is that

[0064] A moisture-curing reactive polyurethane hot melt adhesive is prepared by weighing, by weight, 20 parts of polyether polyol, 30 parts of polyester polyol and 36 parts of isocyanate.

[0065] Table 1 Main components and preparation parameters of polyurethane hot melt adhesive.

[0066]

[0067] According to HG / T 3716-2003 and GB / T 7122-1996, the hot melt adhesives prepared in Examples 1 to 3 and Comparative Examples 1 to 7 were tested for open time and peel strength. The test results are shown in Table 2.

[0068] Table 2 Hot melt adhesive performance test results of Examples 1 to 3 and Comparative Examples 1 to 7.

[0069] Example Opening hours / s Peel strength / MPa Example 1 29 36 Example 2 31 42 Example 3 32 48 Comparative Example 1 89 26 Comparative Example 2 96 25 Comparative Example 3 101 28 Comparative Example 4 62 33 Comparative Example 5 78 31 Comparative Example 6 22 26 Comparative Example 7 182 23

[0070] From the above embodiments and comparative examples, it can be seen that the present application selects raw materials with simple preparation process and more advantageous cost, with polyether polyol, polyester polyol, isocyanate and tackifying resin as main materials, and adds catalyst, chain extender, coupling agent and other auxiliary materials, to design and prepare a low-cost, moisture-curing reactive polyurethane hot melt adhesive (PUR) with an open time of 25 to 35 seconds, and high peel strength after curing, which can fully meet the operational requirements of automatic edge sealing of furniture.

[0071] Through Examples 1 to 3, it can be known that the open time gradually increases. It is believed that this is mainly because under the condition that the total amount of polyether polyol and polyester polyol accounts for a similar proportion, as the isocyanate content increases, the residual NCO content gradually increases, which increases the NCO reaction consumption time and causes the open time to increase. And through Comparative Example 7, it can be known that when the isocyanate accounts for too much, the open time increases significantly. It is believed that when the polyether polyol and polyester polyol that can react with isocyanate are insufficient, the excess isocyanate can only react and solidify with the moisture in the environment, thereby significantly extending the open time. Moreover, due to the decrease in the content of polyether polyol and polyester polyol, the cross-linked network structure formed by the reaction with isocyanate also decreases, resulting in a decrease in peel strength. Therefore, according to Examples 1 to 3 and Comparative Example 7, it can be known that the preferred ratio of the polyol composition (referring to the mixture of polyether polyol and polyester polyol) to isocyanate is (55 to 59): (23 to 27).

[0072] Through Examples 1 to 3 and Comparative Examples 1 to 3, it can be known that polyether polyol, polyester polyol, isocyanate and tackifying resin have an optimal ratio range, and when isocyanate is added in excess, the residual NCO content is relatively large, which increases the NCO reaction consumption time, that is, the open time of the hot melt adhesive is significantly increased, and in actual use, due to the reduced addition ratio of the tackifying resin, the viscosity of the hot melt adhesive is reduced, the coating property of the hot melt adhesive is reduced, the amount of glue per unit area is reduced, and the peel strength after curing is reduced.

[0073] Through Example 1 and Comparative Examples 4 and 5, it can be known that the open time of Comparative Examples 4 and 5 is longer than that of Example 1, and the peel strength is also reduced. Analysis shows that this is mainly because the polyether polyol and polyester polyol with a functionality of 3.0 used in Example 1 react with isocyanate to cure faster under air humidity conditions, which shortens the open time, and the high-functionality polyol reacts with isocyanate to form a more complex cross-linked structure, which meets the peel strength requirement after furniture edge sealing. Therefore, when Comparative Examples 4 and 5 use polyether polyols and polyester polyols with lower functionality, the hot melt adhesive curing reaction speed is slower, which increases the open time of the hot melt adhesive, and the cross-linked structure after the reaction is simpler than that of Example 1, and the peel strength is also reduced.

[0074] Through Example 1 and Comparative Example 6, it can be known that the open time and peel strength of Comparative Example 6 are significantly reduced. Analysis shows that this is mainly because the polyol composition contains more water, which reacts with the isocyanate added later, consumes part of the isocyanate content, resulting in a decrease in the effective amount of isocyanate and a decrease in the reaction time of the later isocyanate, so the open time is significantly reduced. In addition, due to the decrease in the effective isocyanate content, the cross-linked network structure formed by the reaction with the polyol composition is also reduced, resulting in a decrease in the peel strength.

[0075] The above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the scope of protection of the present invention.

Claims

1. A moisture curing reactive polyurethane hot melt adhesive, characterized in that: The hot melt adhesive comprises the following components by weight:

2. A moisture curing reactive polyurethane hot melt adhesive according to claim 1, characterized in that: The hydroxyl value of the polyether polyol is 30-500 mgKOH / g, and the functionality is 3.0; the hydroxyl value of the polyester polyol is 30-500 mgKOH / g, and the functionality is 3.

0.

3. The moisture-curing reactive polyurethane hot melt adhesive according to claim 1, characterized in that: The polyether polyol includes one or two of 310, 330N or 3050 produced by Langfang Quanzhen Chemical Development Co., Ltd.

4. The moisture-curing reactive polyurethane hot melt adhesive according to claim 1, characterized in that: The polyester polyol includes one or more of PL5601, PL1201 or white polyester produced by Qingdao Ruinuo Chemical Co., Ltd.

5. The moisture curing reactive polyurethane hot melt adhesive according to claim 1, characterized in that: The isocyanate includes diisocyanate; Preferably, the isocyanate includes one or more of MDI, TDI, HDI or IPDI.

6. The moisture-curing reactive polyurethane hot melt adhesive according to claim 1, characterized in that: The tackifying resin includes one or both of rosin resin and terpene resin.

7. The moisture-curing reactive polyurethane hot melt adhesive according to claim 1, characterized in that: The catalyst includes one or more of bismorpholine diethyl ether, triethylenediamine or dibutyltin dilaurate.

8. The moisture-curing reactive polyurethane hot melt adhesive according to claim 1, characterized in that: The chain extender includes 1,4-butanediol, ethylene glycol or trimethylolpropane; the coupling agent is a silane coupling agent, preferably KH550 from Langfang Quanzhen Chemical Development Co., Ltd.

9. A method for preparing the moisture-curing reactive polyurethane hot melt adhesive according to any one of claims 1 to 8, characterized in that: The preparation method comprises the following steps: Step 1: mixing the polyether polyol and the polyester polyol, stirring, heating, and vacuum dehydrating to obtain a polyol composition; Step 2: mixing the polyol composition and the isocyanate to obtain a prepolymer; Step 3: adding the tackifying resin, the catalyst, the chain extender and the coupling agent to the prepolymer, and mixing them evenly to obtain the hot melt adhesive.

10. The preparation method according to claim 9, characterized in that: The water content of the polyol composition is less than 0.015%.

Citation Information

Cited By

  • Non-aqueous reaction type two-component polyurethane grouting material as well as preparation method and application thereof

    CN121427048A