Polyurethane hot melt adhesive as well as preparation method and application thereof
Through the combination of polyether diol, polyester diol and other materials, a polyurethane hot melt adhesive with high initial viscosity and low activity was prepared, which solved the solution of the hot melt adhesive for car lamps between high initial viscosity and low activity. The problem has achieved efficient bonding and low reaction activity, avoided blockage in production, and improved production efficiency and cost-effectiveness.
Patent Information
- Application Number
- CN202411093536.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-09
AI Technical Summary
The hot melt adhesive for existing car lights is difficult to take into account both high initial adhesiveness and low activity, which can easily lead to plate crust and pipeline blockage, affecting production efficiency and cost.
Using a combination of polyether diol, polyester diol, hydroxyl-terminated polybutadiene, isocyanate, polyolefin, tackifying resin and adhesive-promoting agent, high-primary preparation is prepared through specific ratios and process treatments. Viscous, low-reactive polyurethane hot melt adhesive.
The high initial bonding strength and low reaction activity of hot melt adhesive for car lights is achieved, the pressure plate crust and pipeline blockage is avoided, production efficiency is improved, cost is reduced, and good aging resistance is achieved.
Smart Images

Figure BDA0004987229490000151
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyurethane, and in particular relates to a polyurethane hot melt adhesive and a preparation method and application thereof. Background Art
[0002] The bonding and sealing of car lights is an important part of the manufacturing process of automobile lamps. The bonding of car lights should ensure that the car lights will not have problems such as debonding, water and oil seepage, discoloration and fogging when used in various adverse environments. In traditional car light bonding applications, ordinary hot melt adhesives and two-component silicone adhesives are usually used. Ordinary hot melt adhesives have the advantages of fast curing and good initial adhesion, and are the main adhesives used for traditional car light bonding. However, the main component of this hot melt adhesive is thermoplastic polyolefin, which is very sensitive to temperature changes and easy to flow when heated. At the same time, it is also very sensitive to the penetration of water and gasoline, causing problems such as water leakage and fogging of car lights during use, and even causing the entire car light to be scrapped; on the other hand, the polyolefin hot melt adhesive itself has insufficient adhesion to the polycarbonate material of one of the car light structures, especially the polycarbonate that has been surface hardened and wear-resistant is more likely to debond, which is difficult to meet the user's requirements for the bonding strength of the car lights; although the two-component silicone adhesive has improved in high and low temperature performance, it has poor initial adhesion. After the glue is applied, the device often needs to be placed for several hours and cannot be moved, which occupies the site and prolongs the delivery time. Therefore, the development of new polyurethane hot melt adhesives for car lights has always been a research and development hotspot.
[0003] Reactive polyurethane hot melt adhesive (PUR adhesive for short) is made of a single-component, solvent-free terminal isocyanate prepolymer with corresponding additives; its main component is a terminal isocyanate prepolymer synthesized from polyester polyol and diisocyanate, which can cure quickly after melt application and has good initial adhesive strength; during the post-curing process, moisture diffuses into the adhesive and reacts with the isocyanate group of the prepolymer to form urea, biuret and allophanate, so that the linear prepolymer low molecular weight forms a cross-linked macromolecular structure, thus having better high temperature resistance, solvent resistance and water resistance than traditional hot melt adhesive. Similar to ordinary hot melt adhesive, PUR adhesive is heated and melted by a melter and applied on the headlights, and quickly cooled and cured to achieve a high initial bonding strength, and the adhered parts can be moved, assembled and other operations; then during the storage or transportation of the product, PUR adhesive will continue to react with moisture in the air, further increasing the degree of curing, and become a high-strength, temperature-resistant, and solvent-resistant colloid. Since polyurethane hot melt adhesive has the advantages of both traditional hot melt adhesive and two-component silicone adhesive, it can perfectly solve the contradiction between rapid positioning and high-strength bonding in the bonding of car lights. Therefore, it is an ideal substitute for adhesive used for bonding car lights.
[0004] At present, the performance research on reactive polyurethane hot melt adhesive in the prior art mainly focuses on improving its heat resistance and bonding performance, etc., and the raw materials contain high content of polyester polyol and polyether polyol and contain catalyst; CN108467702A discloses a moisture-curing polyurethane hot melt adhesive for car lights and a preparation method thereof, wherein the polyester polyol in the formula is 10-45 parts, and the catalyst is selected from dibutyltin dilaurate, stannous octoate, lead octoate, etc.; CN103740316A discloses a moisture-curing polyurethane hot melt adhesive for car lights and a preparation method thereof, wherein the polyester polyol is as high as 60-85 parts, and the catalyst is selected from dibutyltin dilaurate, stannous octoate, lead octoate; the high content of polyester polyol and catalyst leads to high activity of the hot melt adhesive for car lights, which reacts quickly with moisture in the air, and is prone to cause plate crusting and pipeline blockage during application, affecting the production rhythm and increasing production costs.
[0005] High initial viscosity, low activity hot melt adhesive for automotive lamps can effectively reduce the crusting of pipelines and pressure plates while ensuring the high efficiency of the automotive lamp assembly line, and reduce pipeline scrapping and shutdown caused by pipeline blockage. There is currently no report on low activity, high initial viscosity hot melt adhesive for automotive lamps. Summary of the invention
[0006] In view of the deficiencies in the prior art, the object of the present invention is to provide a polyurethane hot melt adhesive and a preparation method and application thereof. The polyurethane hot melt adhesive provided by the present invention has the characteristics of high initial adhesion and low activity, and at the same time has excellent adhesion after being fully cured.
[0007] To achieve this object, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides a polyurethane hot melt adhesive. The raw materials for preparing the polyurethane hot melt adhesive include, in parts by weight: 100 parts by weight of polyether diol, 40-100 parts by weight of polyester diol, 10-60 parts by weight of hydroxyl-terminated polybutadiene, 10-50 parts by weight of isocyanate, 100-200 parts by weight of polyolefin, 20-100 parts by weight of tackifying resin and 1-10 parts by weight of adhesion promoter; the tackifying resin includes any one of silane coupling agent modified polyisobutylene, silane coupling agent modified amorphous α-polyolefin or silane coupling agent modified metallocene-catalyzed vinyl copolymer or a combination of at least two thereof.
[0009] The polyurethane hot melt adhesive provided by the present invention has the characteristics of high initial adhesion and low activity through the screening of preparation raw materials, and has higher performance after complete curing; wherein the hydroxyl-terminated polybutadiene can improve the adhesion of the polyurethane hot melt adhesive to the substrate; the polyolefin can reduce the water vapor permeability, thereby reducing the reaction activity and initial adhesion of the polyurethane hot melt adhesive; the tackifying resin can improve the wettability of the polyurethane hot melt adhesive, thereby improving its initial adhesion and adhesion after complete curing.
[0010] The polyester diol is 40-100 parts by weight, for example, it can be 40 parts by weight, 45 parts by weight, 50 parts by weight, 55 parts by weight, 60 parts by weight, 65 parts by weight, 70 parts by weight, 75 parts by weight, 80 parts by weight, 85 parts by weight, 90 parts by weight, 95 parts by weight, 100 parts by weight, etc.
[0011] The hydroxyl-terminated polybutadiene is 10-60 parts by weight, for example, 10 parts by weight, 15 parts by weight, 20 parts by weight, 25 parts by weight, 30 parts by weight, 35 parts by weight, 40 parts by weight, 45 parts by weight, 50 parts by weight, 55 parts by weight, 60 parts by weight, etc.
[0012] The isocyanate is 10-50 parts by weight, for example, 10 parts by weight, 15 parts by weight, 20 parts by weight, 25 parts by weight, 30 parts by weight, 35 parts by weight, 40 parts by weight, 45 parts by weight, 50 parts by weight, etc.
[0013] The polyolefin is 100-200 parts by weight, for example, 100 parts by weight, 110 parts by weight, 120 parts by weight, 130 parts by weight, 140 parts by weight, 150 parts by weight, 160 parts by weight, 170 parts by weight, 180 parts by weight, 190 parts by weight, 200 parts by weight, etc.
[0014] The tackifying resin is 20-100 parts by weight, for example, 20 parts by weight, 30 parts by weight, 40 parts by weight, 50 parts by weight, 60 parts by weight, 70 parts by weight, 80 parts by weight, 90 parts by weight, 100 parts by weight, etc.
[0015] The adhesion promoter is 1-10 parts by weight, for example, 1 part by weight, 2 parts by weight, 3 parts by weight, 4 parts by weight, 5 parts by weight, 6 parts by weight, 7 parts by weight, 8 parts by weight, 9 parts by weight, 10 parts by weight, etc.
[0016] In the present invention, the silane coupling agent modified polyisobutylene can be purchased, for example, it can be purchased from the EPION series of Kaneka Chemical; the silane coupling agent modified amorphous α-polyolefin can be purchased, for example, it can be purchased from VESTOPLAST 206 of Evonik; the silane coupling agent modified metallocene-catalyzed vinyl copolymer can be purchased, for example, it can be purchased from the Si-link series of Dow Chemical.
[0017] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the objectives and beneficial effects of the present invention can be better achieved and realized.
[0018] As a preferred technical solution, the polyether diol includes polyoxypropylene ether diol.
[0019] Preferably, the hydroxyl value of the polyether diol is 25-150 mgKOH / g, for example, it can be 25 mgKOH / g, 30 mgKOH / g, 40 mgKOH / g, 50 mgKOH / g, 60 mgKOH / g, 70 mgKOH / g, 80 mgKOH / g, 90 mgKOH / g, 100 mgKOH / g, 110 mgKOH / g, 120 mgKOH / g, 130 mgKOH / g, 140 mgKOH / g, 150 mgKOH / g, etc.
[0020] In the present invention, the polyether diol can be purchased, for example, DL2000, DL1000, DL4000 from Dongda Chemical, C2010D, C2020, C2030, C2040D, Dow Chemical's VORANOL2110TB, VORANOL2120, VORANOL3000LM, VORANOL4240, VORANOL222-056.
[0021] Preferably, the hydroxyl value of the polyester diol is 10-120 mgKOH / g, for example, it can be 10 mgKOH / g, 20 mgKOH / g, 30 mgKOH / g, 40 mgKOH / g, 50 mgKOH / g, 60 mgKOH / g, 70 mgKOH / g, 80 mgKOH / g, 90 mgKOH / g, 100 mgKOH / g, 110 mgKOH / g, 120 mgKOH / g, etc., and 10-60 mgKOH / g is more preferred.
[0022] Preferably, the melting point of the polyester diol is <70°C, for example, it may be 0°C, 5°C, 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, etc.
[0023] Preferably, the polyester diol is obtained by polycondensation of a dibasic acid and / or anhydride with a diol.
[0024] Preferably, the dibasic acid includes any one or a combination of at least two of adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, terephthalic acid, phthalic acid, isophthalic acid or 1,4-cyclohexanedicarboxylic acid.
[0025] Preferably, the acid anhydride includes any one of phthalic anhydride, adipic anhydride, pimelic anhydride, suberic anhydride, azelaic anhydride, sebacic anhydride, terephthalic anhydride, phthalic anhydride, isophthalic anhydride or 1,4-cyclohexanedicarboxylic anhydride, or a combination of at least two thereof.
[0026] Preferably, the diol includes any one or a combination of at least two of 1,4-butanediol, 1,6-hexanediol, ethylene glycol, neopentyl glycol, diethylene glycol, 1,2-propylene glycol, 2-methylpropylene glycol or 2,2,4-trimethyl-1,3-pentanediol.
[0027] Preferably, the polyester diol comprises a combination of a first polyester diol and a second polyester diol.
[0028] Preferably, the first polyester diol includes any one or a combination of at least two of the polyester diols obtained by polycondensation of a first dibasic acid and / or a first acid anhydride with a first diol.
[0029] Preferably, the first dibasic acid comprises any one of adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, terephthalic acid, phthalic acid, isophthalic acid or 1,4-cyclohexanedicarboxylic acid, or a combination of at least two thereof.
[0030] Preferably, the first anhydride comprises phthalic anhydride.
[0031] Preferably, the first diol includes any one of 1,4-butanediol, 1,6-hexanediol, ethylene glycol, neopentyl glycol, diethylene glycol, 1,2-propylene glycol, 2-methylpropylene glycol or 2,2,4-trimethyl-1,3-pentanediol, or a combination of at least two thereof.
[0032] Preferably, the second polyester diol includes any one or a combination of at least two of the polyester diols obtained by polycondensation of a second dibasic acid and / or a second acid anhydride with a second diol.
[0033] Preferably, the second dibasic acid comprises any one of adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, terephthalic acid, phthalic acid, isophthalic acid or 1,4-cyclohexanedicarboxylic acid, or a combination of at least two thereof.
[0034] Preferably, the second anhydride comprises phthalic anhydride.
[0035] Preferably, the second diol comprises 2,2,4-trimethyl-1,3-pentanediol.
[0036] In the present invention, the polyester diol can be purchased, for example, Dynacoll 7362, Dynacoll 7360, Dynacoll 7363, Dynacoll 7365, Dynacoll 7361, Dynacoll 7381, Dynacoll 7110, Dynacoll 7111, Dynacoll 7130, Dynacoll 7131, Dynacoll 7140, Dynacoll 7150, Dynacoll 7210, Dynacoll 7250, Dynacoll 7230, Dynacoll 7255, Dynacoll 7231, Hooker F-531, F-900, F-970, F-972, F-931, F-932, F-902, F-911, F-5610, F-5630, F-4620, F-4621, F-39030, F-39031, F-37070, F-37033, F-37040, F-4910, F-37030, F-37031, F-37032, FJ-20030, Stepan PH-56, PC-205P-30, PD-56, PC-2072P-30, PC-5000P-30, Huide HDPOL6620.
[0037] Preferably, the number average molecular weight of the hydroxyl-terminated polybutadiene is 1000-5000, for example, 1000, 1200, 1500, 1800, 2000, 2200, 2500, 2800, 3000, 3200, 3500, 3800, 4000, 4200, 4500, 4800, etc.
[0038] Preferably, the hydroxyl value of the hydroxyl-terminated polybutadiene is 20-80 mgKOH / g, for example, 20 mgKOH / g, 25 mgKOH / g, 30 mgKOH / g, 35 mgKOH / g, 40 mgKOH / g, 45 mgKOH / g, 50 mgKOH / g, 55 mgKOH / g, 60 mgKOH / g, 65 mgKOH / g, 70 mgKOH / g, 75 mgKOH / g, 80 mgKOH / g, etc.
[0039] Preferably, the isocyanate comprises toluene diisocyanate and / or diphenylmethane diisocyanate.
[0040] Preferably, the ratio of the total molar amount of hydroxyl groups contained in the polyether diol, polyester diol and hydroxyl-terminated polybutadiene to the molar amount of isocyanate groups contained in the isocyanate is 1:(1.5-2), for example, it can be 1:1.5, 1:1.55, 1:1.6, 1:1.65, 1:1.7, 1:1.75, 1:1.8, 1:1.85, 1:1.9, 1:1.95, 1:2, etc.
[0041] Preferably, the polyolefin comprises an alpha-olefin polymer.
[0042] Preferably, the α-olefin includes any one of ethylene, propylene, 1-butene, isobutylene, 1-pentene, 1-hexene, 1-octene or 4-methyl-1-pentene, or a combination of at least two thereof.
[0043] Preferably, the softening point of the polyolefin is 80-120°C, for example, it may be 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, 120°C, etc.
[0044] Preferably, the melt viscosity of the polyolefin at 190° C. is 2000-30000 mPa.s, for example, 2000 mPa.s, 3000 mPa.s, 4000 mPa.s, 5000 mPa.s, 6000 mPa.s, 7000 mPa.s, 8000 mPa.s, 9000 mPa.s, 10000 mPa.s, 15000 mPa.s, 20000 mPa.s, 25000 mPa.s, 30000 mPa.s, etc.
[0045] Preferably, the polyolefin is an amorphous polyolefin.
[0046] In the present invention, the polyolefin can be purchased. For example, the polyolefin can be selected from Huntsman APAO RT 2535, APAO RT 2585, APAO RT 2715, APAO RT 2730, APAO RT 2732, APAO RT2780, Eastman Aerafin 35, Eastman Aerafin 17, Eastman Aerafin 17M, Eastman Aerafin 180, Eastoflex E1003 Amorphous Polyolefin, Eastoflex E1015 Amorphous Polyolefin, Eastman Aerafin 180M Polymer, Evonik VESTOPLAST 703, VESTOPLAST 704, VESTOPLAST 708, VESTOPLAST 750, VESTOPLAST 408, VESTOPLAST 508, Dow POEAFFINTYGA1900, AFFINTY Any one of AFFINTY GA1950, AFFINTY GA1875, AFFINTY GA8200, AFFINTY GA8407, AFFINTY GA1000R, AFFINTY GA9807, AFFINTY GA9817, or a combination of at least two of them.
[0047] Preferably, the softening point of the tackifying resin is 80-120°C, for example, it may be 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, 120°C, etc.
[0048] Preferably, the melt viscosity of the tackifying resin at 190° C. is 3000-10000 mPa.s, for example, 3000 mPa.s, 4000 mPa.s, 5000 mPa.s, 6000 mPa.s, 7000 mPa.s, 8000 mPa.s, 9000 mPa.s, 10000 mPa.s, etc.
[0049] Preferably, the adhesion promoter includes any one of bis-(γ-trimethoxysilylpropyl)amine, γ-mercaptopropyltrimethoxysilane, γ-glycidyloxypropyltrimethoxysilane, γ-isocyanatepropyltrimethoxysilane or N-phenyl-γ-aminopropyltrimethoxysilane, or a combination of at least two thereof.
[0050] Preferably, in parts by weight, the raw materials for preparing the polyurethane hot melt adhesive further include 0.1-1.5 parts by weight of an antioxidant and 0.1-100 parts by weight of carbon black.
[0051] The antioxidant is 0.1-1.5 parts by weight, for example, it can be 0.1 parts by weight, 0.2 parts by weight, 0.3 parts by weight, 0.4 parts by weight, 0.5 parts by weight, 0.6 parts by weight, 0.7 parts by weight, 0.8 parts by weight, 0.9 parts by weight, 1 part by weight, 1.1 parts by weight, 1.2 parts by weight, 1.3 parts by weight, 1.4 parts by weight, 1.5 parts by weight, etc.
[0052] The carbon black is 0.1-100 parts by weight, for example, it can be 0.1 parts by weight, 0.5 parts by weight, 1 parts by weight, 5 parts by weight, 10 parts by weight, 20 parts by weight, 30 parts by weight, 40 parts by weight, 50 parts by weight, 60 parts by weight, 70 parts by weight, 80 parts by weight, 90 parts by weight, 100 parts by weight, etc.; in the present invention, the light resistance of the polyurethane hot melt adhesive can be improved by carbon black.
[0053] Preferably, the antioxidant comprises an aromatic amine antioxidant and / or a hindered phenol antioxidant.
[0054] In the present invention, the antioxidant can be purchased. For example, the antioxidant is selected from any one of RIANOX 1010, RIANOX 1076, RIANOX 1790, RIANOX 168, RIANOX 626, RIANOX DSTP and RIANOXDLTP, or a combination of at least two thereof.
[0055] Preferably, the pH value of the carbon black is >7.5, for example, it can be 7.6, 7.8, 7.9, 8, 8.1, 8.2, 8.4, 8.6, 8.8, 9, 9.2, 9.5, 10, 10.5, 11, 12, 13, 14, etc.
[0056] Preferably, the specific surface area of the carbon black is >100m 2 / g, for example, 101m 2 / g、105m 2 / g, 110m 2 / g, 120m 2 / g, 130m 2 / g, 140m 2 / g, 150m 2 / g, 160m 2 / g, 170m 2 / g, 180m 2 / g, 190m 2 / g, 200m 2 / g, 250m 2 / g、300m 2 / g, 350m 2 / g, etc.
[0057] In a second aspect, the present invention provides a method for preparing the polyurethane hot melt adhesive as described in the first aspect, the preparation method comprising:
[0058] The polyurethane hot melt adhesive is obtained by reacting polyether diol, polyester diol, hydroxyl-terminated polybutadiene, isocyanate, polyolefin, tackifying resin and adhesion promoter.
[0059] Preferably, the preparation method specifically comprises:
[0060] The polyether diol, the polyester diol, the hydroxyl-terminated polybutadiene, the polyolefin and the tackifying resin are mixed, and then the isocyanate is added to carry out the first step reaction; the adhesion promoter is added to the reaction system to carry out the second step reaction to obtain the polyurethane hot melt adhesive.
[0061] Preferably, the mixed material further comprises an antioxidant and carbon black.
[0062] Preferably, the step of vacuum dehydration is further included after the mixing is completed.
[0063] Preferably, the vacuum dehydration is carried out at 110-130°C, for example, 110°C, 112°C, 114°C, 116°C, 118°C, 120°C, 122°C, 124°C, 126°C, 128°C, 130°C, etc.
[0064] Preferably, the vacuum dehydration time is 1-3 h, for example, it can be 1 h, 1.2 h, 1.4 h, 1.6 h, 1.8 h, 2 h, 2.2 h, 2.4 h, 2.6 h, 2.8 h, 3 h, etc.
[0065] Preferably, the first step reaction is carried out under an inert gas atmosphere.
[0066] Preferably, the temperature of the first step reaction is 80-100°C, for example, it can be 80°C, 82°C, 84°C, 86°C, 88°C, 90°C, 92°C, 94°C, 96°C, 98°C, 100°C, etc.
[0067] Preferably, the first step reaction time is 1-3 h, for example, it can be 1 h, 1.2 h, 1.4 h, 1.6 h, 1.8 h, 2 h, 2.2 h, 2.4 h, 2.6 h, 2.8 h, 3 h, etc.
[0068] Preferably, the second step reaction is carried out under vacuum conditions.
[0069] Preferably, the temperature of the second step reaction is 90-120°C, for example, it can be 90°C, 92°C, 94°C, 96°C, 98°C, 100°C, 102°C, 104°C, 106°C, 108°C, 110°C, 112°C, 114°C, 116°C, 118°C, 120°C, etc.
[0070] Preferably, the time of the second step reaction is 20-60 min, for example, it can be 20 min, 22 min, 25 min, 30 min, 32 min, 35 min, 40 min, 45 min, 48 min, 50 min, 52 min, 55 min, 58 min, 60 min, etc.
[0071] In a third aspect, the present invention provides a polyurethane hot melt adhesive as described in the first aspect, which is used as a hot melt adhesive for vehicle lamps.
[0072] Compared with the prior art, the present invention has the following beneficial effects:
[0073] The polyurethane hot melt adhesive provided by the present invention has high initial viscosity, low activity, is not easy to clog equipment, and has good aging resistance. After being fully cured, it has excellent adhesion and can be used as a hot melt adhesive for car lights. The curing speed of the polyurethane hot melt adhesive provided by the present invention is 0.2-0.3mm / 24h, the initial bonding strength after 10min is 0.61-0.76MPa, and the bonding strength after being fully cured is 2.1-2.3MPa. DETAILED DESCRIPTION
[0074] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0075] The sources of some components in the embodiments and comparative examples are as follows:
[0076] (1) Polyether diol: DL2000 (hydroxyl value 56 mgKOH / g) and DL1000 (hydroxyl value 112 mgKOH / g) from Dongda Chemical;
[0077] (2) Polyester diols: Evonik Dynacoll 7360 (hydroxyl value 32 mgKOH / g, melting point 59°C), Evonik Dynacoll 7361 (hydroxyl value 12.5 mgKOH / g, melting point 63°C), Huide HDPOL 6620 (hydroxyl value 56 mgKOH / g, melting point 60°C);
[0078] (3) Hydroxyl-terminated polybutadiene: Total polyBD r45v, hydroxyl value of 35-52 mgKOH / g, number average molecular weight of 2000-3500;
[0079] (4) Amorphous polyolefins: Evonik VESTOPLAST 408 (softening point 118°C, viscosity at 190°C 8000±2000 mPa.s), Evonik VESTOPLAST 508 (softening point 84°C, viscosity at 190°C 8000±2000 mPa.s);
[0080] (5) Tackifying resin silane coupling agent modified amorphous α-polyolefin: Evonik VESTOPLAST 206 (softening point 98°C, viscosity 5000±1000 mPa.s at 190°C);
[0081] (6) MDI: Covestro Desmodur 44C;
[0082] (7) Antioxidants: RIANOX 1010, RIANOX 1076;
[0083] (8) Carbon black: Orion HIBLACK 30 (pH 8.5, specific surface area 110 m 2 / g), Orion PRINTEX90 (pH 9.0, specific surface area 350m 2 / g);
[0084] (9) Adhesion promoter: Evonik MTMO, Dynasylan 1124;
[0085] (10) Acrylic resin: Mitsubishi Chemical BR113, softening point 160°C, Tg 75°C.
[0086] Example 1
[0087] A polyurethane hot melt adhesive, wherein the raw materials for preparing the polyurethane hot melt adhesive include: 100 parts by weight of polyether diol DL2000, 60 parts by weight of polyester diol Dynacoll 7360, 20 parts by weight of hydroxyl-terminated polybutadiene polyBD r45v, 30 parts by weight of MDI, 120 parts by weight of amorphous polyolefin VESTOPLAST 408, 650 parts by weight of VESTOPLAST 20, 100.5 parts by weight of antioxidant RIANOX 10, 10 parts by weight of carbon black HIBLACK 30, and an adhesion promoter MTMO 2 parts by weight;
[0088] The preparation method of the polyurethane hot melt adhesive comprises:
[0089] Add polyether diol DL2000, polyester diol Dynacoll 7360, amorphous polyolefin VESTOPLAST408, hydroxyl-terminated polybutadiene polyBD r45v, carbon black HIBLACK 30, antioxidant RIANOX 1010 and VESTOPLAST206 into the reactor according to the formula amount, heat up to 115-120°C, dehydrate for 2 hours under vacuum degree ≤-0.095MPa to a water content of ≤500ppm, then cool to 80°C, add the formula amount of MDI, heat up to 90°C and react for 2 hours; finally add the formula amount of adhesion promoter MTMO is stirred and dispersed for reaction at 100° C. under vacuum for 1 hour to obtain the polyurethane hot melt adhesive.
[0090] Example 2
[0091] A polyurethane hot melt adhesive, wherein the raw materials for preparing the polyurethane hot melt adhesive include: 100 parts by weight of polyether diol DL2000, 80 parts by weight of polyester diol Dynacoll 7360, 40 parts by weight of hydroxyl-terminated polybutadiene polyBD r45v, 35 parts by weight of MDI, 150 parts by weight of amorphous polyolefin VESTOPLAST 408, 30 parts by weight of VESTOPLAST 206, 101 parts by weight of antioxidant RIANOX 10, 50 parts by weight of carbon black HIBLACK 30, and an adhesion promoter MTMO 5 parts by weight;
[0092] The preparation method of the polyurethane hot melt adhesive comprises:
[0093] Add polyether diol DL2000, polyester diol Dynacoll 7360, amorphous polyolefin VESTOPLAST408, hydroxyl-terminated polybutadiene polyBD r45v, carbon black HIBLACK 30, antioxidant RIANOX 1010 and VESTOPLAST206 into the reactor according to the formula amount, heat up to 120-125°C, dehydrate for 1.5 hours under vacuum degree ≤-0.095MPa to a water content of ≤500ppm, then cool to 90°C, add the formula amount of MDI, heat up to 95°C and react for 1.5 hours; finally, add the formula amount of adhesion promoter MTMO is stirred and dispersed for reaction at 100° C. under vacuum for 30 minutes to obtain the polyurethane hot melt adhesive.
[0094] Example 3
[0095] A polyurethane hot melt adhesive, wherein the raw materials for preparing the polyurethane hot melt adhesive include: 100 parts by weight of polyether diol DL2000, 2045 parts by weight of polyester diol HDPOL66, 55 parts by weight of hydroxyl-terminated polybutadiene polyBD r45v, 40 parts by weight of MDI, 180 parts by weight of amorphous polyolefin VESTOPLAST 508, 670 parts by weight of VESTOPLAST 20, 761.4 parts by weight of antioxidant RIANOX 10, 90 parts by weight of carbon black PRINTEX 9, and 1248 parts by weight of adhesion promoter Dynasylan;
[0096] The preparation method of the polyurethane hot melt adhesive comprises:
[0097] The polyether diol DL2000, polyester diol HDPOL6620, amorphous polyolefin VESTOPLAST 508, hydroxyl-terminated polybutadiene polyBD r45v, carbon black PRINTEX 90, antioxidant RIANOX 1076 and VESTOPLAST 206 are added into a reaction kettle according to the formula amount, the temperature is raised to 125-130°C, and dehydrated for 1.5 hours under the condition of vacuum degree ≤-0.095MPa to a water content of ≤500ppm, then the temperature is lowered to 95°C, the formula amount of MDI is added, the temperature is raised to 100°C and reacted for 1.5 hours; finally, the formula amount of adhesion promoter Dynasylan 1124 is added, and the mixture is stirred and dispersed at 110°C under vacuum for 30 minutes to obtain the polyurethane hot melt adhesive.
[0098] Example 4
[0099] A polyurethane hot melt adhesive, wherein the raw materials for preparing the polyurethane hot melt adhesive include: 100 parts by weight of polyether diol DL1000, 145 parts by weight of polyester diol Dynacoll 736, 35 parts by weight of hydroxyl-terminated polybutadiene polyBD r45v, 48 parts by weight of MDI, 140 parts by weight of amorphous polyolefin VESTOPLAST 508, 680 parts by weight of VESTOPLAST 20, 760.7 parts by weight of antioxidant RIANOX 10, 90 parts by weight of carbon black HIBLACK 30, and an adhesion promoter MTMO 4 parts by weight;
[0100] The preparation method of the polyurethane hot melt adhesive comprises:
[0101] Add polyether diol DL1000, polyester diol Dynacoll 7361, amorphous polyolefin VESTOPLAST508, hydroxyl-terminated polybutadiene polyBD r45v, carbon black HIBLACK 30, antioxidant RIANOX 1076 and VESTOPLAST206 into the reactor according to the formula amount, heat up to 120-125°C, dehydrate for 2 hours under vacuum degree ≤-0.095MPa to a water content of ≤500ppm, then cool to 90°C, add the formula amount of MDI, heat up to 95°C and react for 2 hours; finally, add the formula amount of adhesion promoter MTMO, stirring and dispersing reaction at 120° C. under vacuum for 30 minutes to obtain the polyurethane hot melt adhesive.
[0102] Comparative Example 1
[0103] A polyurethane hot melt adhesive and a preparation method thereof, which differs from Example 1 only in that the amount of polyester diol Dynacoll 7360 used is 20 parts by weight, and the remaining raw materials, process parameters and steps are the same as those in Example 1.
[0104] Comparative Example 2
[0105] A polyurethane hot melt adhesive and a preparation method thereof, which differs from Example 1 only in that the amount of polyester diol Dynacoll 7360 used is 130 parts by weight, and the remaining raw materials, process parameters and steps are the same as those in Example 1.
[0106] Comparative Example 3
[0107] A polyurethane hot melt adhesive and a preparation method thereof, which differs from Example 1 only in that VESTOPLAST206 is not used, and the remaining raw materials, process parameters and steps are the same as those of Example 1.
[0108] Comparative Example 4
[0109] A polyurethane hot melt adhesive and a preparation method thereof, which differs from Example 1 only in that hydroxyl-terminated polybutadiene polyBD r45v is not used, and the remaining raw materials, process parameters and steps are the same as those of Example 1.
[0110] Comparative Example 5
[0111] A polyurethane hot melt adhesive and a preparation method thereof, which differs from Example 1 only in that the amorphous polyolefin VESTOPLAST 408 is not used, and the remaining raw materials, process parameters and steps are the same as those of Example 1.
[0112] Comparative Example 6
[0113] A polyurethane hot melt adhesive and a preparation method thereof, which differs from Example 1 only in that VESTOPLAST 206 is replaced by acrylic resin BR113 in equal amounts, and the remaining raw materials, process parameters and steps are the same as those in Example 1.
[0114] Performance Testing
[0115] (1) Curing speed: Determination of curing degree of sealant according to GB / T 32369-2015, wedge groove method;
[0116] (2) Initial bonding strength: Samples were prepared and tested according to GB / T 7124-2008 to test the initial bonding strength of polyurethane hot melt adhesives; the tensile shear strength was tested after the samples were placed under 25°C / 50% RH conditions for 30 min; bonding substrates: PP-T40 / PC;
[0117] (3) Bond strength after full curing: Samples were prepared and tested according to GB / T 7124-2008 to test the bond strength of polyurethane hot melt adhesive after full curing; the tensile shear strength was tested after the samples were cured at 25°C / 50% RH for 14 days; bonding substrate: PP-T40 / PC;
[0118] The polyurethane hot melt adhesives provided in Examples 1-4 and Comparative Examples 1-6 were tested according to the above test method. The test results are shown in Table 1:
[0119] Table 1
[0120]
[0121] It can be seen from Table 1 that the polyurethane hot melt adhesive provided by the embodiment of the present invention has the characteristics of low activity (slow curing speed), high initial bonding strength, and high bonding strength after complete curing.
[0122] Compared with Example 1, the initial adhesion and bonding strength after complete curing of the polyurethane hot melt adhesive provided in Comparative Example 1 are significantly reduced, and the amount of crystalline polyester diol used has an important influence on the initial adhesion and bonding strength after complete curing of the polyurethane hot melt adhesive.
[0123] Compared with Example 1, the activity (curing speed) of the polyurethane hot melt adhesive provided in Comparative Example 2 is significantly improved, and the bonding strength decreases significantly after complete curing. This is because the excessive crystalline polyester diol destroys the compatibility of the system, resulting in a decrease in the bonding strength of the polyurethane hot melt adhesive after complete curing.
[0124] Compared with Example 1, the activity (curing speed) of the polyurethane hot melt adhesive provided in Comparative Example 3 is significantly improved, and the initial tack and bonding strength after complete curing are significantly reduced. The addition of tackifying resin has an important influence on maintaining the low activity, high initial tack and bonding strength after complete curing of the polyurethane hot melt adhesive.
[0125] Compared with Example 1, the activity (curing speed) of the polyurethane hot melt adhesive provided in Comparative Example 4 is significantly improved, and the bonding strength is significantly reduced after complete curing. The hydroxyl-terminated polybutadiene has an important influence on maintaining the low activity of the polyurethane hot melt adhesive and the bonding strength after complete curing.
[0126] Compared with Example 1, the activity (curing speed) of the polyurethane hot melt adhesive provided in Comparative Example 5 is significantly improved, and the initial adhesion and bonding strength after complete curing are significantly reduced. Polyolefin has an important influence on maintaining the low activity, high initial adhesion and bonding strength after complete curing of the polyurethane hot melt adhesive.
[0127] Compared with Example 1, the activity (curing speed) of the polyurethane hot melt adhesive provided in Comparative Example 6 is significantly improved, and the bonding strength decreases significantly after complete curing. The type of tackifying resin has an important influence on maintaining the low activity, high initial adhesion and bonding strength after complete curing of the polyurethane hot melt adhesive.
[0128] The applicant declares that the present invention uses the above-mentioned embodiments to illustrate the polyurethane hot melt adhesive and its preparation method and application, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A polyurethane hot melt adhesive, It is characterized in that The raw materials for preparing the polyurethane hot melt adhesive include, by weight: 100 parts by weight of polyether diol, 40-100 parts by weight of polyester diol, 10-60 parts by weight of hydroxyl-terminated polybutadiene, 10-50 parts by weight of isocyanate, 100-200 parts by weight of polyolefin, 20-100 parts by weight of tackifying resin and 1-10 parts by weight of adhesion promoter; The tackifying resin includes any one of silane coupling agent modified polyisobutylene, silane coupling agent modified amorphous alpha polyolefin or silane coupling agent modified metallocene catalyzed vinyl copolymer or a combination of at least two thereof.
2. The polyurethane hot melt adhesive according to claim 1, It is characterized in that The polyether diol includes polyoxypropylene ether diol; Preferably, the hydroxyl value of the polyether diol is 25-150 mgKOH / g.
3. The polyurethane hot melt adhesive according to claim 1 or 2, It is characterized in that The hydroxyl value of the polyester diol is 10-120 mgKOH / g; Preferably, the melting point of the polyester diol is <70°C; Preferably, the polyester diol is obtained by polycondensation of a dibasic acid and / or anhydride with a diol; Preferably, the dibasic acid comprises any one or a combination of at least two of adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, terephthalic acid, phthalic acid, isophthalic acid or 1,4-cyclohexanedicarboxylic acid; Preferably, the acid anhydride comprises any one of phthalic anhydride, adipic anhydride, pimelic anhydride, suberic anhydride, azelaic anhydride, sebacic anhydride, terephthalic anhydride, phthalic anhydride, isophthalic anhydride or 1,4-cyclohexanedicarboxylic anhydride, or a combination of at least two thereof; Preferably, the diol includes any one or a combination of at least two of 1,4-butanediol, 1,6-hexanediol, ethylene glycol, neopentyl glycol, diethylene glycol, 1,2-propylene glycol, 2-methylpropylene glycol or 2,2,4-trimethyl-1,3-pentanediol.
4. The polyurethane hot melt adhesive according to any one of claims 1 to 3, It is characterized in that The number average molecular weight of the hydroxyl-terminated polybutadiene is 1000-5000; Preferably, the hydroxyl value of the hydroxyl-terminated polybutadiene is 20-80 mgKOH / g; Preferably, the isocyanate comprises toluene diisocyanate and / or diphenylmethane diisocyanate; Preferably, the ratio of the total molar amount of hydroxyl groups contained in the polyether diol, polyester diol and hydroxyl-terminated polybutadiene to the molar amount of isocyanate groups contained in the isocyanate is 1:(1.5-2).
5. The polyurethane hot melt adhesive according to any one of claims 1 to 4, It is characterized in that The polyolefin comprises an alpha-olefin polymer; Preferably, the α-olefin includes any one or a combination of at least two of ethylene, propylene, 1-butene, isobutylene, 1-pentene, 1-hexene, 1-octene or 4-methyl-1-pentene; Preferably, the softening point of the polyolefin is 80-120°C; Preferably, the melt viscosity of the polyolefin at 190° C. is 2000-30000 mPa.s.
6. The polyurethane hot melt adhesive according to any one of claims 1 to 5, It is characterized in that The softening point of the tackifying resin is 80-120°C; Preferably, the melt viscosity of the tackifying resin at 190° C. is 3000-10000 mPa.s.
7. The polyurethane hot melt adhesive according to any one of claims 1 to 6, It is characterized in that The adhesion promoter includes any one of bis-(γ-trimethoxysilylpropyl)amine, γ-mercaptopropyltrimethoxysilane, γ-glycidyloxypropyltrimethoxysilane, γ-isocyanatepropyltrimethoxysilane or N-phenyl-γ-aminopropyltrimethoxysilane, or a combination of at least two thereof; Preferably, the raw materials for preparing the polyurethane hot melt adhesive further include 0.1-1.5 parts by weight of an antioxidant and 0.1-100 parts by weight of carbon black, in parts by weight; Preferably, the pH value of the carbon black is >7.5; Preferably, the specific surface area of the carbon black is >100m 2 / g.
8. A method for preparing the polyurethane hot melt adhesive according to any one of claims 1 to 7, It is characterized in that The preparation method comprises: The polyurethane hot melt adhesive is obtained by reacting polyether diol, polyester diol, hydroxyl-terminated polybutadiene, isocyanate, polyolefin, tackifying resin and adhesion promoter.
9. The preparation method according to claim 8, It is characterized in that The preparation method specifically comprises: The polyether diol, the polyester diol, the hydroxyl-terminated polybutadiene, the polyolefin and the tackifying resin are mixed, and then the isocyanate is added to carry out a first step reaction; the adhesion promoter is added to the reaction system to carry out a second step reaction to obtain the polyurethane hot melt adhesive; Preferably, the mixed material further comprises an antioxidant and carbon black; Preferably, after the mixing is completed, a vacuum dehydration step is also included; Preferably, the vacuum dehydration is carried out at 110-130°C; Preferably, the vacuum dehydration time is 1-3h; Preferably, the first step reaction is carried out under an inert gas atmosphere; Preferably, the temperature of the first step reaction is 80-100°C; Preferably, the first step reaction time is 1-3h; Preferably, the second step reaction is carried out under vacuum conditions; Preferably, the temperature of the second step reaction is 90-120°C; Preferably, the second step reaction time is 20-60 min.
10. A polyurethane hot melt adhesive as claimed in any one of claims 1 to 7 used as a hot melt adhesive for vehicle lamps.
Citation Information
Patent Citations
Polyurethane hot melt adhesive for car lamp
CN110819292A
Polyolefin modified reactive polyurethane hot melt adhesive and preparation method thereof
CN113322043A
Reactive polyurethane hot melt adhesive for sealing car lamp and preparation method thereof
CN115595109A
Polyurethane hot melt adhesive and preparation method thereof
CN116144311A
Polyurethane hot melt adhesive as well as preparation method and application thereof
CN118374254A