Damp-heat-aging-resistant storage alcohol type silicone sealant and preparation method thereof

By using α,ω-dihydroxypolydimethylsiloxane and modified nano-calcium carbonate in dealcohol type silicone sealant, combined with organic titanium catalyst and protective agent of tributyl citrate sodium hexametaphosphate, the solution is solved The problem of poor odor and water resistance during storage and aging is achieved, and stable curing and environmentally friendly sealing effects under high temperature and high humidity conditions are achieved.

CN118931476APending Publication Date: 2024-11-12HUBEI XINGRUI SILICON MATERIAL CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411072515.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-12-14
Filing Date
2024-08-06
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing dealcoholized silicone sealant has odor problems, poor water resistance and insufficient catalyst stability during storage and aging, which affects its environmental protection and use effect.

Method used

Using α,ω-dihydroxypolydimethylsiloxane as base gel, modified nano calcium carbonate as thixotropic agent, organic titanium as catalyst, and a mixture of tributyl citrate and sodium hexametaphosphate as catalyst Protective agent, combined with γ-aminopropyltriethoxysilane, improves the stability and performance of the catalyst.

Benefits of technology

It achieves odorless and heat-resistant aging performance improvement, extends the storage time of the catalyst, and maintains the curing capacity under high temperature and high humidity conditions, improving the environmental protection and use effect of the product.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a damp-heat aging resistant storage alcohol type silicone sealant and a preparation method of the damp-heat aging resistant storage alcohol type silicone sealant. The invention discloses a damp-heat aging resistant alcohol storage type silicone sealant and a preparation method thereof. The damp-heat aging resistant alcohol storage type silicone sealant is prepared from the following components in parts by mass: 60-80 parts of alpha, omega-dihydroxy polydimethylsiloxane, 40-60 parts of a plasticizer, 100-200 parts of inorganic filler, 5-15 parts of a cross-linking agent, 2-5 parts of a coupling agent, 0.2-0.8 part of a catalyst protective agent and 1-3 parts of a titanium chelate. After the alcohol type silicone sealant is aged for 7 days at the temperature of 100 DEG C, the alcohol type silicone sealant can still be normally subjected to surface drying and curing, and the mechanical property is basically kept.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of room temperature vulcanized silicone rubber and its production technology, and in particular to a moisture and heat aging resistant storage alcohol type silicone sealant and a preparation method thereof. Background Art

[0002] Dealcoholized silicone sealant is a single-component room temperature vulcanized sealant that relies on moisture in the air to undergo a cross-linking reaction, removes alcohol small molecules, and vulcanizes into an excellent, durable elastic silicone sealant. It has lower VOC emissions than other types, is more environmentally friendly, and is more in line with the country's green development concept. With people's increasing requirements for home decoration quality and their emphasis on health, environmental protection, and safety issues, various decorative products that are non-toxic to the human body and friendly to the environment are gradually gaining favor. At present, the alcohol-based silicone sealant products on the market mainly have the following problems: Patent CN106047273A discloses an alcohol-based sealant, which uses a cyclic silicon nitrogen compound as a stabilizer and a blocked polydimethylsiloxane, which increases the process cost and uses an organotin catalyst as its catalyst. Organic titanium compounds are more environmentally friendly, pollution-free, and more versatile than organic tin compounds. Patent CN102911198A attempts to add linear silazane as a stabilizer, but the stabilizer releases ammonia after the rubber material captures alcohol, which makes the rubber material have a strong ammonia smell and also has the possibility of alkaline corrosion to some coating substrates.

[0003] Patent CN116162438A discloses an alcohol-type silicone sealant. The free alcohol in the rubber material is removed by azeotropic removal of methanol carrier by the present invention, and the obtained dealcoholized RTV-1 silicone rubber is odorless and greatly improves the storage performance of the dealcoholized RTV-1 silicone rubber. However, in the embodiments, fumed silica is often used as a filler, and the test result of the obtained rubber sample is 20LM grade. In addition, the Wacker alcohol-type transparent sealant also has a low modulus, a low tensile strength of the product, and poor water-resistant adhesion. Summary of the invention

[0004] The present invention aims to provide a moisture-heat aging resistant storage alcohol type silicone sealant and a preparation method thereof, using α, ω-dihydroxy polydimethylsiloxane as a base glue, modified nano calcium carbonate as a thixotropic agent, a silane coupling agent as an adhesive, and organic titanium as a catalyst, with the purpose of developing a truly healthy and environmentally friendly sealant product suitable for home decoration. The technical solution of the present invention is as follows: An alcohol-type silicone sealant resistant to moisture and heat aging storage, the alcohol-type silicone sealant comprising the following components in parts by weight: 100 parts by mass of α,ω-dihydroxypolydimethylsiloxane; 40-60 parts by mass of a plasticizer; 100-200 parts by mass of inorganic filler; 5-15 parts by mass of a cross-linking agent; 2-5 parts by mass of a coupling agent; 0.2-0.8 parts by mass of a catalyst protective agent; 1-3 parts by mass of catalyst composition.

[0005] Preferably, the viscosity of the α,ω-dihydroxypolydimethylsiloxane is 20000-80000 mPa.s.

[0006] Preferably, the plasticizer is a mixture of one or more of methyl silicone oil, white oil and dioctyl phthalate.

[0007] Preferably, the inorganic filler is a mixture of one or more of modified nano calcium carbonate, silicon powder, heavy calcium carbonate and fumed silica.

[0008] Preferably, the crosslinking agent is a mixture of one or more of vinyltrimethoxysilane, methyltrimethoxysilane, methyltriethoxysilane and polymethyltriethoxysilane.

[0009] Preferably, the coupling agent is one of γ-aminopropyltriethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, γ-(2,3-epoxypropyloxy)propyltrimethoxysilane, or a mixture of two thereof.

[0010] Preferably, the catalyst protective agent is a mixture of tributyl citrate and sodium hexametaphosphate; preferably, the catalyst protective agent is a mixture of tributyl citrate and sodium hexametaphosphate in a mass ratio of (95-110):3.

[0011] Preferably, the catalyst is diisopropoxytitanium bis(ethyl acetoacetate) chelate, diisopropyl di(acetylacetonato)titanate or ethyl acetoacetate titanium chelate.

[0012] The preparation method of the alcohol-type silicone rubber resistant to moisture and heat aging storage, the method steps are as follows: S1: Place α,ω-dihydroxy polydimethylsiloxane, plasticizer and inorganic filler into a kneader at room temperature and mix evenly, heat to 120°C, set the vacuum degree to less than -0.098Mpa, and dehydrate for two hours to prepare a base material; S2: evenly mix the cross-linking agent, coupling agent and catalyst protective agent to prepare an auxiliary agent; S3: Cool the base material to 70°C, mix it with the additive, vacuumize and stir, then cool it down, add the catalyst, vacuumize and stir; discharge and bottle.

[0013] Preferably, the step S1: heating to 115-125° C., vacuum degree less than -0.098 MPa, dehydration for 1.5-2.5 hours; The step S3: cooling the base material to 65-75° C., mixing with the auxiliary agent, vacuuming and stirring for 25-40 minutes, with the vacuum degree being less than -0.098 Mpa, and then cooling to 25-45° C., adding the catalyst, vacuuming and stirring for 15-25 minutes, with the vacuum degree being less than -0.098 Mpa.

[0014] Preferably, when the catalyst protective agent is a mixture of tributyl citrate and sodium hexametaphosphate in a mass ratio of (95-110):3, the preparation method of the catalyst protective agent is to first heat the tributyl citrate to 115-125°C, add the sodium hexametaphosphate, stir for 1.5-2.5 hours under a vacuum degree of less than -0.098Mpa, cool to 90-100°C, add γ-aminopropyltriethoxysilane, stir under negative pressure for 25-35 minutes, cool and bottle for standby use, and the amount of γ-aminopropyltriethoxysilane added is 3-7% of the mass fraction of the mixture of tributyl citrate and sodium hexametaphosphate.

[0015] The beneficial effects of the present invention are: 1. The present invention does not use a hydroxyl scavenger, but uses a mixture of tributyl citrate and sodium hexametaphosphate as a catalyst stabilizer, thereby reducing the problem of failure of the titanium catalyst after long-term storage or aging, and improving the storage performance of the product.

[0016] 2. The present invention adopts organic titanium as a catalyst and adds a catalyst stabilizer to improve the practical problem of short storage time of traditional organic titanium catalyst. The support glue can still be cured normally after aging for 7 days under double 85 (temperature 85°C, humidity 85%) conditions. DETAILED DESCRIPTION

[0017] The present invention is described in further detail below in conjunction with examples, but embodiments of the present invention are not limited thereto. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art. The test methods for which specific experimental conditions are not specified in the following examples are usually carried out according to conventional experimental conditions or according to the experimental conditions recommended by the manufacturer. Unless otherwise specified, reagents and raw materials used in the present invention can be obtained by commercial means or conventional methods.

[0018] Example 1 The components and weight fractions of the silicone sealant described in the embodiment are detailed in Table 1; the following is a detailed description of the method for preparing an alcohol-type silicone rubber resistant to moisture and heat aging storage, taking the components of sequence number 1 described in Table 1 as an example: at room temperature, 100 parts by weight of α, ω-dihydroxy polydimethylsiloxane, 40 parts by weight of plasticizer, and 120 parts by weight of inorganic filler are put into a kneader and mixed evenly, heated to 120°C, the vacuum degree is less than -0.098Mpa, and dehydrated for two hours to prepare a base material; 14 parts by weight of a cross-linking agent, 5 parts by weight of a coupling agent, and 0.2 parts by weight of a catalyst protective agent are mixed evenly to prepare an auxiliary agent; the base material is cooled to 70°C, mixed with the auxiliary agent, vacuumed and stirred for 30 minutes, the vacuum degree is less than -0.098Mpa, and then cooled to 40°C, 3 parts by weight of a catalyst are added, vacuumed and mixed and stirred for 20 minutes, and the vacuum degree is less than -0.098Mpa; the material is discharged and bottled.

[0019] The inorganic filler is M2 nano calcium carbonate; The plasticizer is 100cs viscosity methyl silicone oil; The crosslinking agent is methyltrimethoxysilane and methyltriethoxysilane; N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane (KH-550) and γ-(2,3-epoxypropyloxy)propyltrimethoxysilane (KH-560) are coupling agents; Ethyl acetoacetate titanium chelate is used as the catalyst.

[0020] The catalyst protective agent of No. 1-5 is tributyl citrate.

[0021] Catalyst protective agent No. 6 is a mixture of tributyl citrate and sodium hexametaphosphate in a mass ratio of (100): (3):.

[0022] When the catalyst protective agent is a mixture of tributyl citrate and sodium hexametaphosphate, first heat tributyl citrate to 120°C, add sodium hexametaphosphate, stir for 2 hours under vacuum degree less than -0.098Mpa, cool to 100°C, add γ-aminopropyl triethoxysilane, stir for 30 minutes under negative pressure, cool and bottle. The mass ratio of tributyl citrate, sodium hexametaphosphate and γ-aminopropyl triethoxysilane is 100:3:5.

[0023] The catalyst protective agent No. 7 is the same as No. 6, except that the preparation method of the auxiliary agent is different, and γ-aminopropyltriethoxysilane is not added when preparing the catalyst protective agent.

[0024] The following Table 2, No. 1-7, shows the test results of various properties of the sealants made of various components. The mechanical properties test was conducted in accordance with GB / T13477.8.

[0025] It can be seen from Table 2 that the alcohol-type silicone rubber resistant to moisture and heat aging storage of the present invention has storage performance. Table 1 Example formulation Serial number 50,000 107 glue / g M2 nano calcium carbonate / g 100cs viscosity methyl silicone oil / g Methyltrimethoxysilane / g Methyltriethoxysilane / g KH-550 / g KH-560 / g Catalyst stabilizer / g Catalyst / g 1 100 120 40 6 8 3.5 1.5 0 3 2 100 120 40 6 8 3.5 1.5 0.2 3 3 100 120 40 6 8 3.5 1.5 0.4 3 4 100 120 40 6 8 3.5 1.5 0.6 3 5 100 120 40 6 8 3.5 1.5 0.8 3 6 100 120 40 6 8 3.5 1.5 0.2 3 7 100 120 40 6 8 3.5 1.5 0.2 3 Table 2 Test results of the embodiment Serial number Surface dry / min 24 hours curing Tensile strength / Mpa Elongation at break / 100% Surface dry after double 85 aging / min Double 85 aging and curing Double 85 tensile strength after aging / Mpa Elongation at break of double 85 after aging / 100% 1 24 √ 1.21 324 71 Unable to solidify / / 2 28 √ 1.19 345 30 √ 0.98 412 3 28 √ 1.20 334 35 √ 0.94 431 4 36 √ 1.20 365 31 √ 0.88 465 5 41 √ 1.16 384 30 √ 0.86 512 6 25 √ 1.24 356 24 √ 1.10 390 7 22 √ 1.20 315 27 √ 0.90 400 It can be seen from Table 1-2 that after adding the prepared catalyst stabilizer, the aging effect of double 85 is better. It can still cure normally after 7 days with little strength loss. As the amount increases, the effect weakens; after adding a mixture of tributyl citrate and sodium hexametaphosphate, the effect is better; after changing the preparation method of the stabilizer, the effect cannot reach the optimal state.

[0026] The technical solution of the present invention is explained through the above embodiments, but the present invention is not limited to the above embodiments, that is, it does not mean that the present invention must rely on the above specific embodiments to be implemented. Any improvements made by technicians in the relevant field based on the present invention, or equivalent replacement of the materials selected by the present invention, etc., fall within the scope of protection of the patent.

Claims

1. An alcohol-type silicone sealant resistant to moisture and heat aging storage, characterized in that: The alcohol-based silicone sealant comprises the following components in parts by weight: 100 parts by mass of α,ω-dihydroxypolydimethylsiloxane; 40-60 parts by mass of a plasticizer; 100-200 parts by mass of inorganic filler; 5-15 parts by mass of a cross-linking agent; 2-5 parts by mass of a coupling agent; 0.2-0.8 parts by mass of a catalyst protective agent; 1-3 parts by mass of catalyst composition.

2. The alcohol-type silicone sealant resistant to moisture and heat aging storage according to claim 1, characterized in that: The viscosity of the α,ω-dihydroxy polydimethylsiloxane is 20000-80000 mPa.s.

3. The alcohol-type silicone sealant resistant to moisture and heat aging storage according to claim 1, characterized in that: The plasticizer is a mixture of one or more of methyl silicone oil, white oil and dioctyl phthalate.

4. The alcohol-type silicone sealant resistant to moisture and heat aging storage according to claim 1, characterized in that: The inorganic filler is a mixture of one or more of modified nano calcium carbonate, silicon powder, heavy calcium carbonate and fumed silica.

5. The alcohol-type silicone sealant resistant to moisture and heat aging storage according to claim 1, characterized in that: The crosslinking agent is a mixture of one or more of vinyl trimethoxy silane, methyl trimethoxy silane, methyl triethoxy silane and polymethyl triethoxy silane.

6. The alcohol-type silicone sealant resistant to moisture and heat aging storage according to claim 1, characterized in that: The coupling agent is one of gamma-aminopropyltriethoxysilane, N-(β-aminoethyl)-gamma-aminopropyltrimethoxysilane and gamma-(2,3-epoxypropoxy)propyltrimethoxysilane or a mixture of two thereof.

7. The alcohol-type silicone sealant resistant to moisture and heat aging storage according to claim 1, characterized in that: The catalyst protective agent is tributyl citrate; Preferably, the catalyst protective agent is a mixture of tributyl citrate and sodium hexametaphosphate in a mass ratio of (95-110):

3.

8. The alcohol-type silicone sealant resistant to moisture and heat aging storage according to claim 1, characterized in that: The catalyst is diisopropoxy titanium bis(ethyl acetoacetate) chelate, di(acetylacetonato)titanate diisopropyl ester or ethyl acetoacetate titanium chelate.

9. The method for preparing the alcohol-type silicone rubber resistant to moisture and heat aging storage according to any one of claims 1 to 8, characterized in that: The method steps are as follows: S1: Place α,ω-dihydroxy polydimethylsiloxane, plasticizer and inorganic filler into a kneader at room temperature and mix evenly, heat to 120°C, set the vacuum degree to less than -0.098Mpa, and dehydrate for two hours to prepare a base material; S2: evenly mix the cross-linking agent, coupling agent and catalyst protective agent to prepare an auxiliary agent; S3: Cool the base material to 70°C, mix it with the additive, vacuumize and stir, then cool it down, add the catalyst, vacuumize and stir; discharge and bottle.

10. The method for preparing the alcohol-type silicone rubber resistant to moisture and heat aging storage according to claim 9, characterized in that: The step S1: heating to 115-125°C, vacuum degree less than -0.098Mpa, dehydrating for 1.5-2.5 hours; The step S3: cooling the base material to 65-75° C., mixing with the auxiliary agent, vacuuming and stirring for 25-40 minutes, with the vacuum degree being less than -0.098 Mpa, and then cooling to 25-45° C., adding the catalyst, vacuuming and stirring for 15-25 minutes, with the vacuum degree being less than -0.098 Mpa.