Magnesium-based thermochemical energy storage material and preparation method thereof
The preparation of nitrate-doped magnesium oxide-based thermochemical energy storage materials through one-step calcination method has solved the problem of cumbersome preparation and poor stability of existing MgO-based materials, achieved efficient thermal energy storage and release, and promoted industrial application.
Patent Information
- Application Number
- CN202411405877.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-10
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-10-10
AI Technical Summary
The preparation process of existing MgO-based thermochemical energy storage materials is cumbersome, resulting in high energy loss and poor cycle stability, limiting their industrial production and application.
The magnesium oxide-based thermochemical energy storage material doped with nitrate is directly prepared from the magnesium precursor by one-step calcination method. The magnesium precursor is mixed with carbonate and nitrate and then calcined in one step to form a nano-scale petal lamellar structure. Improve reaction rate and cycle stability.
The preparation process is simplified, energy loss is reduced, MgO carbonation rate and cycle stability are improved, thermal energy release and storage efficiency is enhanced, and industrial production is promoted.
Smart Images

Figure CN118931507A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to magnesium-based thermochemical energy storage materials, and in particular relates to a magnesium-based thermochemical energy storage material and a preparation method thereof. Background Art
[0002] Among the many energy storage technologies, one very important one is to convert temporarily excess energy into thermal energy for storage. Thermal energy storage is to store heat by using heat storage materials and release energy when needed, which has great development potential. According to different principles, thermal energy storage can generally be divided into sensible heat storage, latent heat storage (phase change heat storage) and thermochemical energy storage. Among them, thermochemical energy storage, as a cutting-edge heat storage technology, is superior to sensible heat and latent heat storage in terms of heat storage temperature and energy storage density. In addition, since thermal energy is stored in the form of chemical energy, zero loss and long-term storage of thermal energy can be achieved in theory.
[0003] As the foundation of thermochemical energy storage technology, thermochemical energy storage materials are the most important components. Among them, the thermochemical heat storage materials of the MgO / MgCO3 system with low cost, wide temperature window, high heat storage density and environmental friendliness are considered to be one of the most promising materials (Formula 1). However, as a solid phase heat storage material, the MgO / MgCO3 system is also limited by factors such as slow reaction rate, weak cycle stability and complex preparation, which is not conducive to large-scale industrial production and application.
[0004] Formula 1 At present, the synthesis method of existing MgO-based thermochemical energy storage materials is mainly prepared by a two-step method. In the first step, MgO is prepared by reacting a magnesium precursor with a precipitant, drying, and calcining. In the second step, a dopant is added to the prepared MgO by a water-soluble method or an alcohol-soluble method, and then dried and calcined again to obtain the final MgO-based thermochemical energy storage material. The preparation process of this method is cumbersome, not only a lot of electrical energy is consumed in the multi-step drying and calcination, but also sample loss is prone to occur during the transfer process. Summary of the invention
[0005] In view of the above technical problems, the present invention provides a magnesium-based thermochemical energy storage material and a preparation method thereof. The present invention directly prepares a nitrate-modified magnesium oxide-based thermochemical energy storage material from a magnesium precursor by a one-step calcination method, thereby reducing the preparation steps, lowering the cost, and improving the MgO carbonation rate and enhancing the cycle stability.
[0006] To achieve the above object, the technical solution of the present invention is: A magnesium-based thermochemical energy storage material, comprising a magnesium oxide matrix and a dopant loaded on the magnesium oxide matrix, wherein the microstructure of the magnesium-based thermochemical energy storage material is a nano-scale petal layer, and the dopant is a nitrate, wherein the nitrate can be in a molten state in the magnesium-based thermochemical energy storage material, and the liquid nitrate can reduce the Mg-O bond energy and accelerate the reaction rate of magnesium oxide and carbon dioxide; The preparation method of the magnesium-based thermochemical energy storage material comprises the following steps: S1: stirring and mixing the magnesium precursor solution and the carbonate solution, filtering after the reaction; S2: stirring and mixing the nitrate solution and the filtered product of step S1, and drying the mixture; S3: placing the mixture dried in step S2 into a high temperature furnace for calcination.
[0007] The magnesium precursor can be magnesium chloride hexahydrate or magnesium nitrate, and the carbonate can be potassium carbonate or sodium carbonate. Due to the reaction chemical formula in the MgO / MgCO3 system, the molar ratio of the magnesium precursor to the carbonate is the same or the carbonate is slightly excessive (for example, within 1.1 times or 1.2 times) to allow the magnesium precursor to react fully.
[0008] The nitrate can be LiNO3, NaNO3, KNO3, LiNO3-NaNO3, NaNO3-KNO3, LiNO3-KNO3, LiNO3-NaNO3-KNO3.
[0009] Preferably, the nitrate is a ternary alkali metal nitrate of LiNO3-NaNO3-KNO3. This alkali metal nitrate is selected because the alkali metal nitrate molten salt has a low melting point and can melt earlier during the heating process, thereby promoting the reaction rate of magnesium oxide.
[0010] The LiNO3-NaNO3-KNO3 mixing ratio can be selected according to the LiNO3-NaNO3-KNO3 phase diagram, as long as it is in a molten state within the working range of the magnesium oxide matrix temperature. Preferably, the molar ratio of the LiNO3-NaNO3-KNO3 is 0.3:0.18:0.52. The nitrate in this ratio is a eutectic LiNO3-NaNO3-KNO3 ternary molten salt with a lower melting point, which can melt earlier and accelerate the reaction rate of magnesium oxide.
[0011] Preferably, the molar ratio of the dopant to the magnesium-based thermochemical energy storage material is 5-20. Experiments have shown that when the surface doping ratio is greater than 20, the reaction rate does not increase but decreases. This may be because the excessively high ratio causes nitrates to block the pores on the surface of magnesium oxide and inhibit the reaction.
[0012] Preferably, the molar ratio of the dopant to the magnesium-based thermochemical energy storage material is 10-20, and more preferably the molar ratio is 20, which promotes higher reaction efficiency.
[0013] Preferably, the calcination temperature in step S3 is 400-450°C, which causes the obtained energy storage material to present a nano-scale petal microporous sheet structure, so that the magnesium-based thermochemical energy storage material can effectively promote the flow of carbon dioxide inside the magnesium oxide during the heat release and storage process, thereby increasing the reaction rate. If the temperature is too low, magnesium oxide cannot be produced by the reaction, and if the temperature is too high, the microscopic morphology of the nano-scale petal microporous sheet cannot be achieved.
[0014] Furthermore, in step S3, the mixture is heated to 450° C. in a high-temperature furnace at a heating rate of 5° C. / min and kept at that temperature for 4 hours for calcination.
[0015] Based on the same inventive concept, the present invention provides a method for preparing a magnesium-based thermochemical energy storage material, comprising the following steps: S1: stirring and mixing the magnesium precursor solution and the carbonate solution, filtering after the reaction; S2: stirring and mixing the nitrate solution and the filtered product of step S1, and drying the mixture; S3: placing the dried mixture in step S2 into a high-temperature furnace for calcination to obtain the magnesium-based thermochemical energy storage material; The magnesium-based thermochemical energy storage material comprises a magnesium oxide matrix and a dopant loaded on the magnesium oxide matrix. The microstructure of the magnesium-based thermochemical energy storage material is a nano-scale petal layer, and the dopant is nitrate.
[0016] Preferably, the step S1 specifically comprises preparing a solution of a magnesium precursor and a carbonate in a molar ratio of 1:1, and pouring the carbonate solution into the magnesium precursor solution, stirring, reacting, and filtering.
[0017] The magnesium precursor is MgCl2·6H2O, and the carbonate is Na2CO3. In addition, the magnesium precursor may also be magnesium nitrate, and the carbonate may also be potassium carbonate.
[0018] Preferably, the calcination temperature in step S3 is 400-450°C, which causes the obtained energy storage material to present a nano-scale petal microporous sheet structure, so that the magnesium-based thermochemical energy storage material can effectively promote the flow of carbon dioxide inside the magnesium oxide during the heat release and storage process, thereby increasing the reaction rate. If the temperature is too low, magnesium oxide cannot be produced by the reaction, and if the temperature is too high, the microscopic morphology of the nano-scale petal microporous sheet cannot be achieved.
[0019] Furthermore, in step S3, the mixture is heated to 450° C. in a high-temperature furnace at a heating rate of 5° C. / min and kept at that temperature for 4 hours for calcination.
[0020] Preferably, the step S2 specifically comprises preparing a nitrate solution of LiNO3-NaNO3-KNO3 alkali metal nitrates in a molar ratio of 0.3:0.18:0.52, stirring and mixing the nitrate solution with the filtered product of step S1, and drying the mixture at 105-120°C for 12-24h.
[0021] Preferably, in step S2, nitrate accounting for 5-20 mol % of the magnesium-based thermochemical energy storage material is weighed to prepare a nitrate solution.
[0022] Due to the adoption of the above technical solution, the present invention has the following advantages and positive effects compared with the prior art: The magnesium-based thermochemical energy storage material provided by the present invention directly obtains the nitrate-doped energy storage material by one-step calcination of the magnesium precursor, and the doping of nitrate can weaken the internal lattice energy of magnesium oxide, accelerate the reaction rate, and increase the energy density and cycle stability. Further, the nitrate-doped magnesium-based thermochemical energy storage material is directly prepared from the magnesium precursor by a one-step calcination method, which greatly simplifies the preparation process, reduces the energy loss in the preparation process, and effectively promotes industrial production.
[0023] In another embodiment of the present invention, the calcination temperature is strictly controlled so that the final material presents a nano-scale petal-like microporous lamellar structure, which can effectively promote the flow of carbon dioxide inside the magnesium oxide during the heat release and storage process of the magnesium-based thermochemical energy storage material, thereby increasing the reaction rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a microscopic scanning electron microscope image of the magnesium-based thermochemical energy storage material prepared in Example 1 of the present invention; Figure 2 This is an energy storage density curve diagram of the magnesium-based thermochemical energy storage material prepared in Example 1 of the present invention; Figure 3 This is a cyclic stability diagram of the magnesium-based thermochemical energy storage material prepared in Example 1 of the present invention; Figure 4 This is an energy storage density curve diagram of the magnesium-based thermochemical energy storage material prepared in Example 2 of the present invention; Figure 5 This is a cyclic stability diagram of the magnesium-based thermochemical energy storage material prepared in Example 2 of the present invention; Figure 6 This is an energy storage density curve diagram of the magnesium-based thermochemical energy storage material prepared in Example 3 of the present invention; Figure 7This is an energy storage density curve of the material MgO-1 prepared in Comparative Example 1 of the present invention; Figure 8 This is a cyclic stability diagram of the material MgO-1 prepared in Comparative Example 1 of the present invention; Fig. 9 This is an energy storage density curve of the material MgO-2 prepared in Comparative Example 2 of the present invention; Fig.10 This is a cyclic stability diagram of the material MgO-2 prepared in Comparative Example 2 of the present invention; Fig.11 This is a microscopic scanning electron microscope image of MgO-3 prepared in Comparative Example 3 of the present invention; Fig.12 This is an energy storage density curve diagram of the material MgO-3 prepared in Comparative Example 3 of the present invention; Fig.13 This is a cyclic stability diagram of the material MgO-3 prepared in Comparative Example 3 of the present invention; Fig.14 This is a microscopic scanning electron microscope image of MgO-4 prepared in Comparative Example 4 of the present invention; Fig.15 This is an energy storage density curve of the material MgO-4 prepared in Comparative Example 4 of the present invention.
[0025] Note: Figure 2 , 4 , 6, 7, 9, 12, 15, the English ordinate of the energy storage density curve graph means heat storage density, and the English abscissa means time; Figure 3 , 5 , 8, 10, and 13. The English vertical axis of the cyclic stability diagrams means the heat storage density, and the English horizontal axis means the number of cycles. DETAILED DESCRIPTION
[0026] The magnesium-based thermochemical energy storage material and the preparation method thereof proposed by the present invention are further described in detail below in conjunction with the accompanying drawings and specific embodiments. The advantages and features of the present invention will become more apparent from the following description.
[0027] In the following embodiments of the present invention, the magnesium-based thermochemical energy storage material is named AMN X -MgO, AMN is the abbreviation of LiNO3-NaNO3-KNO3, X is the molar ratio of molten salt in MgO-based thermochemical energy storage materials, and X is between 0-20.
[0028] Example 1 AMN 10 The preparation method of -MgO comprises: S1: Weigh an equivalent mass of MgCl2·6H2O and Na2CO3 in a molar ratio of 1:1 and put them into beakers respectively, and add 100 mL of deionized water to prepare solutions with concentrations of 0.6 mol / L and 0.8 mol / L; put the beaker containing the Na2CO3 solution on a magnetic stirrer and pour the pre-prepared MgCl2·6H2O solution into it, stir at room temperature for 1 hour, and filter after the reaction; S2: Weigh 10 mol% of alkali metal nitrate (LiNO3-NaNO3-KNO3=0.3:0.18:0.52) into a beaker, add 40 mL of deionized water to prepare an inorganic salt solution; add the inorganic salt solution to the filtered product of step S1, and stir evenly in a magnetic stirrer; dry the evenly stirred mixture in a 120°C oven for 12 hours; S3: The dried mixture was placed in a muffle furnace and calcined for 4 hours at 450°C to obtain a nitrate-doped MgO-based thermochemical energy storage material (heating rate 5°C / min); the cooled sample was ground into powder in an agate mortar and sealed in a sealed bag, named AMN 10 -MgO for subsequent use.
[0029] Thermogravimetric analysis instrument was used to test the energy storage density of MgO-based thermochemical energy storage materials. 10 mg of material was weighed and placed in an alumina crucible and placed in a thermogravimetric analyzer; pure N2 was introduced into the thermogravimetric analyzer at a gas flow rate of 50 mL / min, and the temperature was raised to 350°C at a heating rate of 10°C / min at room temperature for 10 minutes to remove moisture and impurity gases; the gas was switched to a mixture of CO2 and N2 (40 vol% CO2 and 60 vol% N2 mixed atmosphere, flow rate of 50 mL / min), and the temperature was kept at 350°C for 120 minutes (30 minutes for the cyclic stability test); the gas was switched to pure N2 (flow rate of 50 mL / min), and the temperature was raised to 450°C for 10 minutes. This reciprocating cycle can test the energy storage density and cyclic stability of MgO-based thermochemical energy storage materials.
[0030] According to the mass change data during the test, the energy storage density of MgO-based thermochemical energy storage materials is calculated: , The AMN prepared in Example 1 10 -MgO for microstructure and thermochemical energy storage density testing. Figure 1 As shown, Figure 1 After calcination in step S3, the MgO-based thermochemical energy storage material presents a nano-level petal-like layer structure, and each layer has a large number of pores. This special structure is conducive to the flow of CO2 in the material and accelerates the reaction rate. The test results of energy storage density are as follows Figure 2 and Figure 3 As shown in the figure, the energy storage density can reach 1710.07 kJ / kg in 120 minutes. Under the condition of 30 minutes carbonation reaction, the energy storage density decays by 17.41% after 10 rapid cycles, and the final energy storage density is 479.36 kJ / kg.
[0031] Example 2 AMN 20 The preparation method of -MgO comprises: S1: Weigh an equivalent mass of MgCl2·6H2O and Na2CO3 in a molar ratio of 1:1 and put them into beakers respectively, and add 100 mL of deionized water to prepare solutions with concentrations of 0.6 mol / L and 0.8 mol / L; put the beaker containing the Na2CO3 solution on a magnetic stirrer and pour the pre-prepared MgCl2·6H2O solution into it, stir at room temperature for 1 hour, and filter after the reaction; S2: Weigh 20 mol% of alkali metal nitrate (LiNO3-NaNO3-KNO3=0.3:0.18:0.52) into a beaker, add 40 mL of deionized water to prepare an inorganic salt aqueous solution; add the inorganic salt aqueous solution to the above-mentioned filtered product, and then stir it in a magnetic stirrer; put the stirred mixture into a 120°C oven and dry it for 12 hours; S3: The dried mixture was placed in a muffle furnace at 450°C and calcined for 4 hours to obtain the molten salt-doped MgO-based thermochemical energy storage material (heating rate 5°C / min); the cooled sample was ground into powder in an agate mortar and sealed in a sealed bag, named AMN 20 -MgO for subsequent use.
[0032] AMN was analyzed by thermogravimetric analysis. 20 -MgO material was tested for energy storage density. Weigh 10 mg of material and put it into an alumina crucible, and place it in a thermogravimetric analyzer; introduce pure N2 into the thermogravimetric analyzer at a gas flow rate of 50 mL / min, and heat it to 350°C at a heating rate of 10°C / min at room temperature for 10 min to remove moisture and impurity gases; switch the gas to a mixture of CO2 and N2 (40 vol% CO2 and 60 vol% N2 mixed atmosphere, flow rate of 50 mL / min), and keep it at 350°C for 120 minutes (30 minutes for cyclic stability test); switch the gas to pure N2 (flow rate of 50 mL / min), heat it to 450°C and keep it at a constant temperature for 10 minutes. Repeating this cycle can test AMN 20 -Energy storage density and cycling stability of MgO.
[0033] The AMN prepared in Example 2 20-MgO was tested for thermochemical energy storage density. The test results of energy storage density are as follows Figure 4 and Figure 5 As shown in the figure, the energy storage density can reach 1625.67 kJ / kg in 120 minutes. Under the condition of 30 minutes carbonation reaction, the energy storage density decays by 18.18% after 10 rapid cycles, and the final energy storage density is 450.28 kJ / kg.
[0034] Example 3 S1: Weigh an equivalent mass of MgCl2·6H2O and Na2CO3 in a molar ratio of 1:1 and put them into beakers respectively, and add 100 mL of deionized water to prepare solutions with concentrations of 0.6 mol / L and 0.8 mol / L; put the beaker containing the Na2CO3 solution on a magnetic stirrer and pour the pre-prepared MgCl2·6H2O solution into it, stir at room temperature for 1 hour, and filter after the reaction; S2: Weigh 5 mol% of alkali metal nitrate (LiNO3-NaNO3-KNO3=0.3:0.18:0.52) into a beaker, add 40 mL of deionized water to prepare an inorganic salt aqueous solution; add the inorganic salt aqueous solution to the above-mentioned filtered product, and then stir it in a magnetic stirrer; put the stirred mixture into a 120°C oven and dry it for 12 hours; S3: The dried mixture was placed in a muffle furnace at 450°C and calcined for 4 hours to obtain the molten salt-doped MgO-based thermochemical energy storage material (heating rate 5°C / min). The cooled sample was ground into powder in an agate mortar and sealed in a sealed bag, named AMN5-MgO for subsequent use.
[0035] Thermogravimetric analysis was used to test the energy storage density of AMN5-MgO. 10 mg of the material was weighed and placed in an alumina crucible and placed in a thermogravimetric analyzer. Pure N2 was introduced into the thermogravimetric analyzer at a gas flow rate of 50 mL / min. The temperature was raised to 350°C at a heating rate of 10°C / min at room temperature for 10 min to remove moisture and impurity gases. The gas was switched to a mixture of CO2 and N2 (40 vol% CO2 and 60 vol% N2 mixed atmosphere, flow rate of 50 mL / min), and the temperature was kept at 350°C for 120 minutes (30 minutes for the cyclic stability test). The gas was switched to pure N2 (flow rate of 50 mL / min), and the temperature was raised to 450°C for 10 minutes. This reciprocating cycle can test the energy storage density and cyclic stability of the MgO-based adsorbent.
[0036] The AMN5-MgO prepared in Example 3 was subjected to a thermochemical energy storage density test. The test results of the energy storage density are as follows: Figure 6 As shown, the energy storage density can reach 1541.89 kJ / kg in 120 minutes.
[0037] Comparative Example 1 S1: Weigh an equivalent mass of MgCl2·6H2O and Na2CO3 in a molar ratio of 1:1 and put them into beakers respectively, and add 100 mL of deionized water to prepare solutions with concentrations of 0.6 mol / L and 0.8 mol / L; put the beaker containing the Na2CO3 solution on a magnetic stirrer and pour the pre-prepared MgCl2·6H2O solution into it, stir at room temperature for 1 hour, and filter after the reaction; S2: calcining the filtered product in a muffle furnace at 450°C to prepare MgO; S3: Weigh 10 mol% of alkali metal nitrate (LiNO3-NaNO3-KNO3=0.3:0.18:0.52) into a beaker, add 40 mL of deionized water to prepare an inorganic salt aqueous solution; add the inorganic salt aqueous solution to the MgO prepared above, and stir evenly in a magnetic stirrer; put the evenly stirred mixture into a 120°C oven and dry it for 12 hours; S4: The dried mixture was placed in a muffle furnace at 450°C and calcined for 4 hours to obtain a sample (heating rate 5°C / min). The cooled sample was ground into powder in an agate mortar and sealed in a sealed bag and named MgO-1 for subsequent use.
[0038] Thermogravimetric analysis instrument was used to test the energy storage density of MgO-1 material. 10 mg of material was weighed and placed in an alumina crucible, and then placed in a thermogravimetric analyzer; pure N2 was introduced into the thermogravimetric analyzer at a gas flow rate of 50 mL / min, and the temperature was raised to 350°C at a heating rate of 10°C / min at room temperature for 10 minutes to remove moisture and impurity gases; the gas was switched to a mixture of CO2 and N2 (40 vol% CO2 and 60 vol% N2 mixed atmosphere, flow rate of 50 mL / min), and the temperature was kept at 350°C for 120 minutes (30 minutes for the cyclic stability test); the gas was switched to pure N2 (flow rate of 50 mL / min), and the temperature was raised to 450°C for 10 minutes. The energy storage density and cyclic stability of MgO-1 can be tested by repeating the cycle.
[0039] The MgO-1 prepared in Example 1 was subjected to a thermochemical energy storage density test. The test results of the energy storage density are as follows: Figure 7 and Figure 8 As shown in the figure, the energy storage density can reach 863.91 kJ / kg in 120 minutes. Under the condition of 30 minutes carbonation reaction, the energy storage density decays by 34.92% after 10 rapid cycles, and the final energy storage density is 276.81 kJ / kg.
[0040] Comparative Example 2: S1: Weigh an equivalent mass of MgCl2·6H2O and Na2CO3 in a molar ratio of 1:1 and put them into beakers respectively, and add 100 mL of deionized water to prepare solutions with concentrations of 0.6 mol / L and 0.8 mol / L; put the beaker containing the Na2CO3 solution on a magnetic stirrer and pour the pre-prepared MgCl2·6H2O solution into it, stir at room temperature for 1 hour, and filter after the reaction; S2: calcining the filtered product in a muffle furnace at 450°C to prepare MgO; S3: Weigh 20 mol% of alkali metal nitrate (LiNO3-NaNO3-KNO3=0.3:0.18:0.52) into a beaker, add 40 mL of deionized water to prepare an inorganic salt aqueous solution; add the inorganic salt aqueous solution to the MgO prepared above, and stir evenly in a magnetic stirrer; put the evenly stirred mixture into a 120°C oven and dry it for 12 hours; S4: The dried mixture was placed in a muffle furnace at 450°C and calcined for 4 hours to obtain a sample (heating rate 5°C / min). The cooled sample was ground into powder in an agate mortar and sealed in a sealed bag and named MgO-2 for subsequent use.
[0041] Thermogravimetric analysis instrument was used to test the energy storage density of MgO-2 material. 10 mg of material was weighed and placed in an alumina crucible, which was then placed in a thermogravimetric analyzer. Pure N2 was introduced into the thermogravimetric analyzer at a gas flow rate of 50 mL / min, and the temperature was raised to 350°C at a heating rate of 10°C / min at room temperature for 10 minutes to remove moisture and impurity gases. The gas was switched to a mixture of CO2 and N2 (40 vol% CO2 and 60 vol% N2 mixed atmosphere, flow rate of 50 mL / min), and the temperature was kept at 350°C for 120 minutes. The gas was switched to pure N2 (flow rate of 50 mL / min), and the temperature was raised to 450°C for 10 minutes.
[0042] The MgO-2 prepared in Example 2 was subjected to a thermochemical energy storage density test. The test results of the energy storage density are as follows: Fig. 9 and Fig.10 As shown in the figure, the energy storage density can reach 1045.96 kJ / kg in 120 minutes. Under the condition of 30 minutes carbonation reaction, the energy storage density decays by 33.92% after 10 rapid cycles, and the final energy storage density is 382.91 kJ / kg.
[0043] Comparative Example 3 Weigh an equivalent mass of MgCl2·6H2O and Na2CO3 in a molar ratio of 1:1 and put them into a beaker, add 100 mL of deionized water to prepare solutions with concentrations of 0.6 mol / L and 0.8 mol / L; place the beaker containing the Na2CO3 solution on a magnetic stirrer and pour in the pre-prepared MgCl2·6H2O solution, stir at room temperature for 1 hour, and filter after the reaction; weigh 10 mol% of alkali metal nitrate (LiNO3-NaNO3-KNO3=0.3:0.18:0.52) and put it into a beaker, add 40 mL of deionized water was used to prepare an inorganic salt aqueous solution; the inorganic salt aqueous solution was added to the above-mentioned filtered product, and then placed in a magnetic stirrer for stirring; the stirred mixture was placed in a 120°C oven for drying for 12 hours; the dried mixture was placed in a 500°C muffle furnace and calcined for 4 hours to obtain a molten salt-doped MgO-based thermochemical energy storage material (heating rate 5°C / min); the cooled sample was placed in an agate mortar and ground into powder, placed in a sealed bag and sealed, named MgO-3 for subsequent use.
[0044] Thermogravimetric analysis was used to test the energy storage density of MgO-based thermochemical energy storage materials. 10 mg of material was weighed and placed in an alumina crucible and placed in a thermogravimetric analyzer; pure N2 was introduced into the thermogravimetric analyzer at a gas flow rate of 50 mL / min, and the temperature was raised to 350°C at a heating rate of 10°C / min at room temperature for 10 minutes to remove moisture and impurity gases; the gas was switched to a mixture of CO2 and N2 (40 vol% CO2 and 60 vol% N2 mixed atmosphere, flow rate of 50 mL / min), and the temperature was kept at 350°C for 120 minutes (30 minutes for the cyclic stability test); the gas was switched to pure N2 (flow rate of 50 mL / min), and the temperature was raised to 450°C for 10 minutes. This reciprocating cycle can test the energy storage density and cyclic stability of the MgO-based adsorbent.
[0045] The MgO-3 prepared in Example 3 was subjected to microscopic morphology analysis and thermochemical energy storage density test. Fig.11 The microscopic morphology of MgO-3 is shown in the figure. It can be seen from the figure that the petal-shaped structure of the product obtained is destroyed under high-temperature calcination, and irregular nano-flakes are presented, which is not conducive to reacting with CO2. The test results of energy storage density are shown in Fig.12 and Fig.13 As shown, the energy storage density is 971.48 kJ / kg in 120 minutes. Under the condition of 30 minutes carbonation reaction, the energy storage density decays by 55% after 10 rapid cycles, and the final energy storage density is 220.36 kJ / kg.
[0046] Comparative Example 4 The raw materials used in this comparative example are exactly the same as those in Example 1, and the preparation method is also the same. The difference from Example 1 is that in step S2, the inorganic salt water prepared with alkali metal salt is not mixed with the filtered product in step S1, and the filtered product is only dried, and then the calcination in step S3 is continued. Therefore, no doping nitrate is added in this comparative example, and the obtained product is named MgO-4. The microscopic morphology of the prepared MgO-4 is as follows Fig.14 The energy storage density of MgO-4 was tested using the same thermogravimetric analyzer and the same experimental conditions as in Example 1. The results are as follows: Fig.15 As shown in the figure, it can be seen that the energy storage density is only 118.31 kJ / kg at 120 minutes, and the energy storage density is around 10 kJ / kg in the first 40 minutes.
[0047] Comparing Example 1 with Comparative Example 1, and Example 2 with Comparative Example 2, it is shown that only by adopting the one-step calcination preparation method of the present invention can a magnesium oxide-based thermochemical energy storage material with higher energy density and higher cycle stability be obtained; in Example 1 and Comparative Example 4, in the same time, the energy storage density of Comparative Example 4 is very low, and the reaction rate is extremely low, the reaction rate of Comparative Example 4 is very low, and the reaction rate of Example 1 is very fast, and thus the energy storage density is large, indicating that doping with nitrate can accelerate the reaction rate; compared with Comparative Example 3, Example 1 strictly controls the calcination temperature to obtain higher energy storage density and cycle stability; compared with Comparative Examples 3 and 4, it can be seen that simultaneous control of temperature and doping with nitrate can obtain stable Figure 1 The microscopic morphology shown. Therefore, through the one-step calcination preparation method of the present invention, a magnesium oxide-based thermochemical energy storage material with higher energy density and higher cycle stability is obtained. Therefore, the magnesium-based thermochemical energy storage material obtained by the preparation method of the present invention not only improves the reaction rate of magnesium oxide, enhances energy density and cycle stability, but also greatly simplifies the preparation process, reduces energy loss in the preparation process, reduces costs, and effectively promotes industrial production.
[0048] The embodiments of the present invention are described in detail above in conjunction with the accompanying drawings, but the present invention is not limited to the above embodiments. Even if various changes are made to the present invention, if these changes fall within the scope of the claims of the present invention and their equivalents, they still fall within the protection scope of the present invention.
Claims
1. A magnesium-based thermochemical energy storage material, characterized in that: The magnesium-based thermochemical energy storage material comprises a magnesium oxide matrix and a dopant loaded on the magnesium oxide matrix, the microstructure of the magnesium-based thermochemical energy storage material is a nano-scale petal layer, and the dopant is a nitrate; The preparation method of the magnesium-based thermochemical energy storage material comprises the following steps: S1: stirring and mixing the magnesium precursor solution and the carbonate solution, filtering after the reaction; S2: stirring and mixing the nitrate solution and the filtered product of step S1, and drying the mixture; S3: placing the mixture dried in step S2 into a high temperature furnace for calcination.
2. The magnesium-based thermochemical energy storage material according to claim 1, characterized in that: The nitrate is LiNO3-NaNO3-KNO3 ternary alkali metal nitrate.
3. The magnesium-based thermochemical energy storage material according to claim 2, characterized in that: The molar ratio of LiNO3-NaNO3-KNO3 is 0.3:0.18:0.
52.
4. The magnesium-based thermochemical energy storage material according to claim 1, characterized in that: The molar ratio of the dopant to the magnesium-based thermochemical energy storage material is 5-20.
5. The magnesium-based thermochemical energy storage material according to claim 4, characterized in that: The molar ratio of the dopant to the magnesium-based thermochemical energy storage material is 10-20.
6. The magnesium-based thermochemical energy storage material according to claim 1, characterized in that: The calcination temperature in step S3 is 400-450°C.
7. The magnesium-based thermochemical energy storage material according to claim 6, characterized in that: In step S3, the mixture is heated to 450° C. in a high-temperature furnace at a heating rate of 5° C. / min and kept at this temperature for 4 hours for calcination.
8. A method for preparing a magnesium-based thermochemical energy storage material, characterized in that: The following steps are involved: S1: stirring and mixing the magnesium precursor solution and the carbonate solution, filtering after the reaction; S2: stirring and mixing the nitrate solution and the filtered product of step S1, and drying the mixture; S3: placing the dried mixture in step S2 into a high-temperature furnace for calcination to obtain the magnesium-based thermochemical energy storage material; The magnesium-based thermochemical energy storage material comprises a magnesium oxide matrix and a dopant loaded on the magnesium oxide matrix. The microstructure of the magnesium-based thermochemical energy storage material is a nano-scale petal layer, and the dopant is nitrate.
9. The method for preparing a magnesium-based thermochemical energy storage material according to claim 8, characterized in that: The calcination temperature in step S3 is 400-450°C.
10. The method for preparing the magnesium-based thermochemical energy storage material according to claim 9, characterized in that: In step S3, the mixture is heated to 450° C. in a high-temperature furnace at a heating rate of 5° C. / min and kept at this temperature for 4 hours for calcination.
11. The method for preparing a magnesium-based thermochemical energy storage material according to claim 8, characterized in that: The step S2 specifically includes preparing a nitrate solution from LiNO3-NaNO3-KNO3 alkali metal nitrates in a molar ratio of 0.3:0.18:0.52, stirring and mixing the nitrate solution with the filtered product of step S1, and drying the mixture at 105-120° C. for 12-24 hours.
12. The method for preparing a magnesium-based thermochemical energy storage material according to claim 8 or 11, characterized in that: In the step S2, nitrate accounting for 5-20 mol % of the magnesium-based thermochemical energy storage material is weighed to prepare a nitrate solution.
Citation Information
Patent Citations
CO2 absorbent as well as preparation method and application method thereof
CN105664708A
High-heat-conductivity MgO doped molten nitrate heat-transfer and heat-storing material as well as in-situ generation method and application thereof
CN108003847A
Chemical heat storage and release material with high heat storage and release density and preparation method thereof
CN111961449A
MgO-based thermochemical energy storage material and preparation method thereof
CN113403040A
Method for preparing porous calcium-based material from eggshell and application of porous calcium-based material in thermochemical energy storage