Preparation of long afterglow nano material with non-thermal coupling energy level ratio sensing performance
By preparing long afterglow nanomaterials with non-thermal coupling energy level ratio sensing performance of rare earth ion doped MgAlyGa2-yO4:xPr3+, the 3P0/1D2 non-thermal coupling energy level transition of Pr3+ was solved by solving the existing medium- and long afterglow nanomaterials in the medium and long afterglow nanomaterials in the art using Pr3+. The problems of poor sensitivity and low accuracy in temperature sensing achieve high sensitivity and accurate temperature measurement in the range of 303-573K.
Patent Information
- Application Number
- CN202410977260.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-12
AI Technical Summary
The existing long afterglow nanomaterials have poor sensitivity, low accuracy, narrow measurement range in temperature sensing, and the fluorescence intensity ratio temperature measurement method based on the thermal coupling energy level has energy gap limitations, resulting in a contradiction between sensitivity and absolute sensitivity.
The co-precipitation method is used to prepare long afterglow nanomaterials with non-thermal coupling energy level ratio sensing performance of rare earth ion-doped non-thermal coupling energy level transitions in Pr3+ to achieve a range of 303-573K The fluorescence intensity ratio temperature measurement avoids the overlapping problems of energy transfer and energy spectrum.
It improves the sensitivity and signal recognition capabilities of temperature sensing, realizes accurate temperature measurement in a wide temperature range, solves the problems of poor sensitivity and low accuracy, and provides new temperature measurement technology ideas.
Smart Images

Figure CN118931530A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of solid luminescence and temperature measurement materials, and specifically relates to the preparation of a rare earth ion-doped long afterglow nanomaterial based on non-thermal coupling energy levels and the application of ratio fluorescence temperature measurement. Background Art
[0002] Temperature is an important parameter in industry and scientific research. Therefore, how to measure temperature conveniently and accurately has become a research hotspot in the field of temperature measurement. At present, there are two main types of temperature sensors used for temperature measurement: contact and non-contact. The contact type (such as thermoresistance thermometer, thermocouple thermometer, etc.) has thermal expansion and first thermoelectric effect, and the non-contact type (such as optical thermometer, full radiation pyrometer, photoelectric pyrometer, etc.) has optical, radiation and photoelectric response. Non-contact temperature measurement based on optical response has significant advantages over traditional contact thermometers: (a) it can monitor the temperature of moving objects or objects that are difficult to access or in dangerous locations; (b) it can measure the temperature of nanoscale devices; (c) it is not subject to electromagnetic interference; (d) the thermal response rate is very fast, which can realize real-time testing. Optical materials used for real-time response temperature measurement may have high sensitivity and appropriate temperature resolution. Modern engineering fields have put forward more requirements for temperature sensors.
[0003] Fluorescence thermometry is an optical thermometry technique that can measure temperature by analyzing the temperature dependence of optical parameters such as fluorescence intensity, fluorescence intensity ratio (FIR), emission position and decay lifetime. Among them, the self-calibrated optical thermometer based on FIR technology is not affected by energy loss, external interference and fluctuations in the density of the excitation source, and is the most promising fluorescence thermometry technology. Since the introduction of FIR technology, the fluorescence intensity ratio thermometry method based on thermal coupling energy levels has been gradually improved. Li et al. used [1,1'-biphenyl]-3,5-dicarboxylic acid (H2BPDA) as a linker and Dy3+ as a single luminescence center to synthesize dysprosium-doped MOF thermometry materials, and used thermal coupling energy levels to monitor the temperature in the range of 303-443K (Journal of Luminescence, 2023, 263:120070). Guan et al. synthesized BaGd2O4:Yb 3+ / Er 3+ Phosphors were studied based on thermal coupling energy levels under 980nm excitation in the range of 298-573K. 2 H 11 / 2 / 4 S 3 / 2 and Er 3+ Stark sublevel 4 F 9 / 2Temperature sensing of the energy level (Spectrochimica Acta Part A: Molecular and Biomolecular Spectroscopy, 2022, 284: 121805). Although these methods can avoid external interference and enhance the stability of fluorescence temperature sensing, it is well known that the energy gap ΔE between the thermal coupling energy levels is 200 cm -1 Up to 2000cm -1 A smaller ΔE may lead to a significant overlap of the two emissions, while a larger ΔE may result in an insufficient number of electrons in the high energy state within a given temperature range, thus resulting in lower sensitivity. Based on the inherent limitation of the small energy gap of the thermal coupling energy level, the simultaneous improvement of relative sensitivity and absolute sensitivity is a contradictory issue.
[0004] As a photoluminescent material, long afterglow nanomaterials can store energy after being excited by external light sources and then
[0005] The light is released in the form of glow. At the same time, the optical properties of long afterglow nanomaterials can be adjusted by doping luminescent centers. Long afterglow nanomaterials can be used as temperature measurement materials. Due to their special optical properties, they can eliminate background fluorescence interference and improve detection accuracy. Doping with rare earth ions can produce multiple emissions within a certain range, thereby realizing FIR temperature measurement at non-thermal coupling energy levels. Compared with FIR technology based on thermal coupling energy levels, FIR technology at non-thermal coupling energy levels is no longer limited by energy gaps. It breaks the limitation of Boltzmann distribution in FIR technology based on thermal coupling energy levels and can achieve high signal discrimination capabilities. Summary of the invention
[0006] The purpose of the present invention is to solve the problems of poor sensitivity, low accuracy and narrow measurement range of long afterglow nanomaterials in the prior art in temperature sensing. The present invention provides a preparation method of a long afterglow material with non-thermal coupling energy level ratio sensing performance and its application in temperature sensing. 3+ When it is used as an emission center, it has a rich energy level structure. 3 P0 / 1 The D2 non-thermal coupling energy level can realize FIR temperature sensing of 303-573K. Compared with thermal coupling energy level temperature sensing, non-thermal coupling energy level temperature measurement can improve both sensitivity and signal recognition capability, providing new ideas for the research field of temperature measurement technology.
[0007] The present invention adopts a coprecipitation method to uniformly mix 0.5 mol / L, 0.5 mol / L, 0.5 mol / L, 0.01 mol / L of aqueous solutions of gallium ions, magnesium ions, aluminum ions and praseodymium ions according to a stoichiometric relationship to obtain MgAl y Ga2-y O4:xPr 3 + A series of long afterglow nanomaterials with the general formula. Under 274nm excitation, the material has Pr 3+ The dual emission phenomenon of a single luminescence center at 494nm and 612nm is different from the non-thermal coupling energy level transition caused by multiple luminescence centers. 3+ of 3 P0 / 1 The D2 non-thermal coupling energy level transition avoids the problems of energy transfer and spectrum overlap between multiple luminescence centers. 3+ of 3 P0 / 1 D2 is the characteristic peak, and a non-thermal coupling energy level ratio temperature sensor is designed to achieve fluorescence temperature measurement at a temperature of 303-573K, which provides a new idea for non-thermal coupling energy level temperature measurement and is more conducive to the practical development of rare earth ions.
[0008] Technical solution of the present invention
[0009] A long afterglow nanomaterial with non-thermal coupled energy level ratio sensing performance of rare earth ion doped photoluminescence thermal quenching effect, the chemical formula of which is MgAl y Ga 2-y O4:xPr 3+ , where x and y are molar quantities, and their ranges are respectively, 0 <x≤1.2%,0≤y≤0.05。
[0010] More preferably, x is 0.05%, 0.1%, 0.3%, 0.6%, 0.9%, 1.2%, and y is 0, 0.02, 0.03, 0.04, 0.05, respectively.
[0011] More preferably, x is 0.1%, y is 0.04, and the long afterglow nanomaterial is MgAl 0.04 Ga 1.96 O4: 0.1% Pr 3+ , a single-phase dual-emission material.
[0012] The present invention also provides a preparation method of a long afterglow nanomaterial with non-thermal coupling energy level ratio sensing performance and its temperature sensing application, and the preparation steps are as follows:
[0013] The coprecipitation method is adopted to prepare gallium oxide, magnesium acetate, aluminum nitrate and praseodymium nitrate in order to prepare 0.5 mol / L, 0.5 mol / L, 0.5 mol / L and 0.01 mol / L aqueous solutions, and the prepared gallium ion, magnesium ion, aluminum ion and praseodymium ion aqueous solutions are mixed according to the general formula MgAl y Ga 2-y O4:xPr 3+The materials are mixed according to the stoichiometric relationship, stirred evenly, and the pH value of the solution is adjusted to 7-11 with concentrated ammonia water. After continuing to stir to make it fully mixed, the mixed solution is centrifuged (centrifuged at a speed of 8000 rpm for 6 minutes), and washed by centrifugation with ultrapure water for multiple times. The obtained centrifugal product is placed in a vacuum drying oven at 120°C for 3 hours. After it is dried, it is ground into powder, transferred to a crucible, and calcined at 700-900°C in a muffle furnace for 1 hour to obtain the rare earth ion-doped long afterglow nanomaterial.
[0014] More preferably, the pH is 7, 8, 9, 10, 11, respectively, and the calcination temperature is 700, 800, 900°C, respectively.
[0015] The present invention also provides an application of the above-mentioned long afterglow nanomaterial with non-thermal coupling energy level ratio sensing performance in temperature sensing, the specific method is to use MgAl y Ga 2-y O4:x%Pr 3+ The launch center Pr 3+ exist 3 P0→ 3 H4 and 1 D2→ 3 The transition process of H4 constitutes a nanomaterial with dual emission at 494 and 612nm under non-thermal coupling energy levels under 274nm excitation, which can be used to prepare ratio temperature sensing elements to achieve real-time and accurate temperature measurement.
[0016] Advantages and beneficial effects of the present invention
[0017] The present invention provides a long afterglow nano material MgAl with non-thermal coupling energy level ratio sensing performance y Ga 2-y O4:xPr 3+ By adjusting the doping amount of Pr and Al ions to control the fluorescence intensity of the nanomaterial, the optimal long afterglow nanomaterial MgAl 0.04 Ga 1.96 O4: 0.1% Pr 3+ A single-phase dual-emission material. Using Pr ions 3 P0 / 1 D2→ 3 The H4 non-thermal coupling energy level transition realizes the fluorescence intensity ratio temperature measurement in the wide temperature detection range of 303-573K, which solves the problems of poor sensitivity, low accuracy and narrow measurement range of long afterglow nanomaterials in temperature sensing in the existing technology. This preparation has application potential in high temperature monitoring such as industrial temperature measurement and electronic temperature measurement. In addition, the preparation method is simple and easy to promote and apply on a large scale, which is expected to provide a new idea for high temperature warning temperature measurement. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 In Example 1, MgGa2O4:xPr 3+ (The legend corresponds to the Pr ion doping amount from top to bottom: 0.05%, 0.1%, 0.3%, 0.6%, 0.9%, 1.2%). Fluorescence emission spectrum of long afterglow material under 274nm excitation.
[0019] Figure 2 In Example 2, MgAl y Ga 2-y O4:xPr 3+ (The legend corresponds from bottom to top to the X-ray diffraction pattern of Pr ion doping amount: 0.1%, Al ion doping amount: 0, 0.02, 0.03, 0.04, 0.05).
[0020] Figure 3 In Example 2, MgAl y Ga 2-y O4:xPr 3+ (The legend corresponds from bottom to top to the Pr ion doping amount: 0.1%, Al ion doping amount: 0, 0.02, 0.03, 0.04, 0.05) Fluorescence emission spectrum of long afterglow material under 274nm excitation.
[0021] Figure 4 In Example 4, the sample MgAl 0.04 Ga 1.96 O4:0.1%Pr 3+ Transmission electron microscopy images of long afterglow nanomaterials.
[0022] Figure 5 In Example 4, the sample MgAl 0.04 Ga 1.96 O4:0.1%Pr 3+ Particle size statistical histogram of long afterglow nanomaterials.
[0023] Figure 6 In Example 4, the sample MgAl 0.04 Ga 1.96 O4:0.1%Pr 3+ Element distribution spectrum of long afterglow nanomaterials.
[0024] Figure 7 In Example 4, the sample MgAl 0.04 Ga 1.96 O4:0.1%Pr 3+ Variable temperature emission spectrum of long afterglow nanomaterials under 274nm excitation.
[0025] Figure 8 In Example 4, the sample MgAl0.04 Ga 1.96 O4:0.1%Pr 3+ Sensitivity of long-lasting nanomaterials.
[0026] Fig. 9 In Example 4, the sample MgAl 0.04 Ga 1.96 O4:0.1%Pr 3+ Diagram of the cooling-heating cycle of long-afterglow nanomaterials. DETAILED DESCRIPTION
[0027] The technical scheme of the present invention is further described in detail and completely in conjunction with the embodiments and the accompanying drawings. However, the following embodiments are only a small part of the embodiments of the present invention and do not represent all the embodiments. All other embodiments based on some embodiments of the present invention, such as those obtained by ordinary technicians in the art without creative work, belong to the scope of protection of the present invention.
[0028] In the following examples, the various raw materials used are all commercially available products known in the art unless otherwise specified. The temperature sensing long afterglow nanomaterial is prepared by the following method: first, gallium oxide, magnesium acetate, aluminum nitrate and praseodymium nitrate are prepared into aqueous solutions with concentrations of 0.5 mol / L, 0.5 mol / L, 0.5 mol / L and 0.01 mol / L, respectively.
[0029] Embodiment 1:
[0030] MgAl 0.04 Ga 1.96 O4:0.1%Pr 3+ Preparation of long afterglow nanometer temperature measuring material, according to MgGa2O4:xPr 3+ (x = 0.05%, 0.1%, 0.3%, 0.6%, 0.9%, 1.2%) molecular formula stoichiometric relationship, the prepared gallium ion, magnesium ion, aluminum ion, praseodymium ion aqueous solution is mixed in a round bottom flask, stirred evenly, the solution pH is adjusted to 9 with concentrated ammonia, stirring is continued, after mixing evenly, centrifuged at 8000rpm for 6min, and then washed three times with pure water. The obtained centrifugal product is placed in a vacuum drying oven at 120℃ for 3h, and after drying, it is ground into powder, transferred to a crucible, placed in a muffle furnace and calcined at 900℃ for 1h, and finely ground again with an agate mortar after cooling to obtain the target product long afterglow nano fluorescent material for temperature monitoring.
[0031] Embodiment 2:
[0032] MgAl 0.04 Ga 1.96 O4:0.1%Pr 3+Preparation of long afterglow nanometer temperature measuring materials, according to MgAl y Ga 2-y O4:005Pr 3+ (x=0.05%,、0.1%、0.3%、0.6%、0.9%、1.2%,y=0、0.02、0.03、0.04、0.05) molecular formula stoichiometric relationship, the prepared gallium ion, magnesium ion, aluminum ion, praseodymium ion aqueous solution are mixed in a round bottom flask, stirred evenly, the solution pH is adjusted to 7 with concentrated ammonia, stirring is continued, after mixing evenly, centrifuged at 8000rpm for 6min, and then washed three times with pure water. The obtained centrifugal product is placed in a vacuum drying oven at 120℃ for 3h, and after drying, it is ground into powder, transferred to a crucible, placed in a muffle furnace and calcined at 900℃ for 1h, and finely ground again with an agate mortar after cooling to obtain the target product long afterglow nano fluorescent material for temperature monitoring.
[0033] Embodiment 3:
[0034] MgAl 0.04 Ga 1.96 O4:0.1%Pr 3+ Preparation of long afterglow nanometer temperature measuring materials, according to MgAl y Ga 2-y O4:xPr 3+ (x=0.05%,、0.1%、0.3%、0.6%、0.9%、1.2%,y=0、0.02、0.03、0.04、0.05) molecular formula stoichiometric relationship, the prepared gallium ion, magnesium ion, aluminum ion, praseodymium ion aqueous solution are mixed in a round bottom flask, stirred evenly, the solution pH is adjusted to 8 with concentrated ammonia, stirring is continued, after mixing evenly, centrifuged at 8000rpm for 6min, and then washed three times with pure water. The obtained centrifugal product is placed in a vacuum drying oven at 120℃ for 3h, and after drying, it is ground into powder, transferred to a crucible, placed in a muffle furnace and calcined at 900℃ for 1h, and finely ground again with an agate mortar after cooling to obtain the target product long afterglow nano fluorescent material for temperature monitoring.
[0035] Embodiment 4:
[0036] MgAl 0.04 Ga 1.96 O4:0.1%Pr 3+ Preparation of long afterglow nanometer temperature measuring materials, according to MgAl y Ga 2-y O4:xPr 3+(x=0.05%,、0.1%、0.3%、0.6%、0.9%、1.2%,y=0、0.02、0.03、0.04、0.05) molecular formula stoichiometric relationship, the prepared gallium ion, magnesium ion, aluminum ion, praseodymium ion aqueous solution are mixed in a round bottom flask, stirred evenly, the solution pH is adjusted to 9 with concentrated ammonia, stirring is continued, after mixing evenly, centrifuged at 8000rpm for 6min, and then washed three times with pure water. The obtained centrifugal product is placed in a vacuum drying oven at 120℃ for 3h, and after drying, it is ground into powder, transferred to a crucible, placed in a muffle furnace and calcined at 900℃ for 1h, and finely ground again with an agate mortar after cooling to obtain the target product long afterglow nano fluorescent material for temperature monitoring.
[0037] Embodiment 5:
[0038] MgAl 0.04 Ga 1.96 O4:0.1%Pr 3+ Preparation of long afterglow nanometer temperature measuring materials, according to MgAl y Ga 2-y O4:xPr 3+ (x=0.05%,、0.1%、0.3%、0.6%、0.9%、1.2%,y=0、0.02、0.03、0.04、0.05) molecular formula stoichiometric relationship, the prepared gallium ion, magnesium ion, aluminum ion, praseodymium ion aqueous solution are mixed in a round bottom flask, stirred evenly, the solution pH is adjusted to 10 with concentrated ammonia, stirring is continued, after mixing evenly, centrifuged at 8000rpm for 6min, and then washed three times with pure water. The obtained centrifugal product is placed in a vacuum drying oven at 120℃ for 3h, and after drying, it is ground into powder, transferred to a crucible, placed in a muffle furnace and calcined at 900℃ for 1h, and finely ground again with an agate mortar after cooling to obtain the target product long afterglow nano fluorescent material for temperature monitoring.
[0039] Embodiment 6:
[0040] MgAl 0.04 Ga 1.96 O4:0.1%Pr 3+ Preparation of long afterglow nanometer temperature measuring materials, according to MgAl y Ga 2-y O4:xPr 3+(x=0.05%,、0.1%、0.3%、0.6%、0.9%、1.2%,y=0、0.02、0.03、0.04、0.05) molecular formula stoichiometric relationship, the prepared gallium ion, magnesium ion, aluminum ion, praseodymium ion aqueous solution are mixed in a round bottom flask, stirred evenly, the solution pH is adjusted to 11 with concentrated ammonia, stirring is continued, after mixing evenly, centrifuged at 8000rpm for 6min, and then washed three times with pure water. The obtained centrifugal product is placed in a vacuum drying oven at 120℃ for 3h, and after drying, it is ground into powder, transferred to a crucible, placed in a muffle furnace and calcined at 900℃ for 1h, and finely ground again with an agate mortar after cooling to obtain the target product long afterglow nano fluorescent material for temperature monitoring.
[0041] Embodiment 7:
[0042] MgAl 0.04 Ga 1.96 O4:0.1%Pr 3+ Preparation of long afterglow nanometer temperature measuring materials, according to MgAl y Ga 2-y O4:xPr 3+ (x=0.05%,、0.1%、0.3%、0.6%、0.9%、1.2%,y=0、0.02、0.03、0.04、0.05) molecular formula stoichiometric relationship, the prepared gallium ion, magnesium ion, aluminum ion, praseodymium ion aqueous solution are mixed in a round bottom flask, stirred evenly, the solution pH is adjusted to 9 with concentrated ammonia, stirring is continued, after mixing evenly, centrifuged at 8000rpm for 6min, and then washed three times with pure water. The obtained centrifugal product is placed in a vacuum drying oven at 120℃ for 3h, and after drying, it is ground into powder, transferred to a crucible, placed in a muffle furnace and calcined at 700℃ for 1h, and finely ground again with an agate mortar after cooling to obtain the target product long afterglow nano fluorescent material for temperature monitoring.
[0043] Embodiment 8:
[0044] MgAl 0.04 Ga 1.96 O4:0.1%Pr 3+ Preparation of long afterglow nanometer temperature measuring materials, according to MgAl y Ga 2-y O4:xPr 3+(x=0.05%,、0.1%、0.3%、0.6%、0.9%、1.2%,y=0、0.02、0.03、0.04、0.05) molecular formula stoichiometric relationship, the prepared gallium ion, magnesium ion, aluminum ion, praseodymium ion aqueous solution are mixed in a round bottom flask, stirred evenly, the solution pH is adjusted to 9 with concentrated ammonia, stirring is continued, after mixing evenly, centrifuged at 8000rpm for 6min, and then washed three times with pure water. The obtained centrifugal product is placed in a vacuum drying oven at 120℃ for 3h, and after drying, it is ground into powder, transferred to a crucible, placed in a muffle furnace and calcined at 800℃ for 1h, and finely ground again with an agate mortar after cooling to obtain the target product long afterglow nano fluorescent material for temperature monitoring.
[0045] Embodiment 9:
[0046] MgAl 0.04 Ga 1.96 O4:0.1%Pr 3+ Preparation of long afterglow nanometer temperature measuring materials, according to MgAl y Ga 2-y O4:xPr 3+ (x = 0.05%, 0.1%, 0.3%, 0.6%, 0.9%, 1.2%, y = 0, 0.02, 0.03, 0.04, 0.05) molecular formula stoichiometric relationship, the prepared gallium ion, magnesium ion, aluminum ion, praseodymium ion aqueous solution is mixed in a round bottom flask, stirred evenly, the solution pH is adjusted to 9 with concentrated ammonia, and continued to stir, after mixing evenly, centrifuged at 8000rpm for 6min, and then washed three times with pure water. The obtained centrifugal product is placed in a vacuum drying oven at 120℃ for 4h, and after drying, it is ground into powder, transferred to a crucible, placed in a muffle furnace and calcined at 900℃ for 1h, and finely ground again with an agate mortar after cooling to obtain the target product long afterglow nano fluorescent material for temperature monitoring.
[0047] Figure 1 is MgGa2O4:xPr 3+ The emission intensity of different doping amounts (x = 0.05%, 0.1%, 0.3%, 0.6%, 0.9%, 1.2%) under fixed excitation at 274nm changes with Pr 3+ The change of doping amount. As shown in the figure, with the doping ion Pr 3+ With the increase of , under 274nm excitation, the position of the emission peak basically does not shift, and when x=0.1%, the fluorescence intensity of the emission peak is the strongest.
[0048] Figure 2 MgAl y Ga 2-y O4:xPr3+ The X-ray diffraction patterns formed by crystal structure identification with different doping amounts (x=0.05%,0.1%,0.3%,0.6%,0.9%,1.2%,y=0,0.02,0.03,0.04,0.05) are completely consistent with the peak position of the standard card PDF#72-1520 of MgGa2O4, and no impurity peaks are introduced, which indicates that the obtained sample is a single-phase sample. 3+ 、Al 3+ The doping does not destroy the crystal structure of MGO.
[0049] Figure 3 MgAl y Ga 2-y O4:xPr 3+ (x=0.05%,0.1%,0.3%,0.6%,0.9%,1.2%,y=0,0.02,0.03,0.04,0.05) The emission intensity of different doping amounts under fixed excitation at 274nm changes with Al 3+ The change of doping amount. As can be seen from the figure, with the doping of ions Al 3+ With the increase of , under 274nm excitation, the position of the emission peak basically does not shift, and the fluorescence intensity of the emission peak is the strongest when y=0.04.
[0050] Figure 4 and Figure 5 The best sample is MgAl 0.04 Ga 1.96 O4:0.1%Pr 3+ Transmission electron microscope spectrum and particle size statistics of long afterglow nanomaterials. From the spectrum, we can see that the size of the prepared material is about 16.23nm.
[0051] Figure 6 The best sample is MgAl 0.04 Ga 1.96 O4:0.1%Pr 3+ The element distribution spectrum of long afterglow nanomaterials shows that elements such as Mg, Ga, Al, O, and Pr are successfully doped into the MgGa2O4 matrix.
[0052] Figure 7 The best sample is MgAl 0.04 Ga 1.96 O4:0.1%Pr 3+ The temperature-dependent emission spectrum of the long afterglow nanomaterial under 274nm excitation. From the spectrum, we can see that with the increase of temperature, the emission peak of the long afterglow nanomaterial at 494nm gradually decreases, and the 612nm peak undergoes a process of first strengthening and then weakening, which is caused by the non-thermal coupling energy level transition and the charge transfer of the metal valence bond.
[0053] Figure 8 The best sample is MgAl 0.04 Ga 1.96 O4:0.1%Pr 3+ The absolute sensitivity and relative sensitivity of the thermometry of the long afterglow nanomaterial based on the non-thermal coupling energy level fluorescence intensity ratio vary with temperature. At 573K, the absolute sensitivity is as high as 2.87%K -1 , at 553K, the best relative sensitivity is 0.91%K -1 .
[0054] Fig. 9 It is the best sample MgAl in this invention. 0.04 Ga 1.96 O4:0.1%Pr 3+ The cooling-heating cycle diagram of the long afterglow nanomaterial shows that during multiple cooling and heating, the fluorescence intensity ratio of the temperature sensing long afterglow nanomaterial at the same temperature remains unchanged, indicating that the temperature sensing long afterglow nanomaterial has good cyclability stability.
Claims
1. A long afterglow nanomaterial with non-thermally coupled energy level ratio sensing performance, whose chemical formula is MgAl y Ga 2-y O4:xPr 3+ ; x and y are molar amounts, and their value ranges are 0 < x ≤ 1.2% and 0 ≤ y ≤ 0.05 respectively. The long afterglow nanomaterial can be repeatedly excited under 274 nm excitation.
2. The long afterglow nanomaterial according to claim 1, characterized in that: x are 0.05%, 0.1%, 0.3%, 0.6%, 0.9% and 1.2% respectively; y are 0, 0.02, 0.03, 0.04 and 0.05 respectively.
3. The long afterglow nanomaterial according to claim 1, characterized in that: The chemical formula of the long afterglow nano material is MgAl 0.04 Ga 1.96 O4: 0.1% Pr 3+ , a single-phase dual-emission material.
4. The preparation method of the long afterglow nanomaterial according to claim 1, characterized in that, The preparation steps are as follows: A co-precipitation preparation method is adopted, wherein the prepared gallium ion, magnesium ion, aluminum ion and praseodymium ion aqueous solutions are mixed according to the general formula and stoichiometric relationship described in claim 1, stirred evenly, and the pH value of the solution is adjusted to 7-11 with concentrated ammonia water. After continuing to stir to make it fully mixed, the mixed solution is centrifuged and washed by centrifugation with ultrapure water. The obtained centrifugal product is placed in a vacuum drying oven at 120° C. for 3 hours, ground into powder after drying, and transferred to a crucible, and calcined at 700-900° C. for 1 hour in a muffle furnace to obtain the rare earth ion-doped long afterglow nanomaterial.
5. The application of the long afterglow nanomaterial according to any one of claims 1 to 3 in non-thermally coupled energy level temperature measurement ratio temperature sensing.
6. The application according to claim 5, characterized in that: Using the launch center Pr 3+ exist 3 P0→ 3 H4 and 1 D2→ 3 The transition process of H4 realizes dual emission of non-thermal coupled energy levels at 494 and 612 nm under 274 nm excitation.
7. The application according to claim 5 or 6, characterized in that: It can be used to prepare ratio temperature sensing elements.
Citation Information
Cited By
Optical temperature sensing fluorescent material as well as preparation method and application thereof
CN120005616A
An optical temperature-sensing fluorescent material, its preparation method and applications
CN120005616B