Metal wire drawing lubricant powder with low caking rate
By using nano-silica powder, lignocellulose and other materials in metal brushed lubricating powder, combined with diatom mud and fatty acid salts, the problem of lubricating powder being prone to clumping is solved, achieving good moisture-proof effect and high application performance.
Patent Information
- Application Number
- CN202410964930.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing metal brushed lubricating powder is prone to agglomeration when encountering small droplets, resulting in poor storage and application effects.
Using nano-silica powder and lignocellulose and other materials, combined with diatom mud, fatty acid salts and sodium nitrite, metal brushed lubricating powder with low agglomeration rate is prepared through drying, breaking, grinding and mixing, to improve its chemical stability. Sex and grainy.
Effectively prevent agglomeration, improve the storage and application effect of lubricating powder, ensure that physical and chemical characteristics are maintained in various environments, and enhance lubricating performance.
Smart Images

Figure CN118931631A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lubricating powders, and in particular relates to a metal wire drawing lubricating powder with a low agglomeration rate. Background Art
[0002] Metal wire drawing is a metal processing technology that forms lines on the metal surface to achieve the effect of decoration and enhance the metal texture. The lines can be straight, random, wavy or spiral, etc., with different visual effects and uses. When drawing metal wires, lubricating powder needs to be applied for lubrication.
[0003] A Chinese patent discloses (CN111808666A) an environmentally friendly wire drawing lubricant powder, which, by weight, comprises 50-80 parts of fatty acid salt, 3-20 parts of lubricating filler, 5-25 parts of auxiliary agent and 1-10 parts of lubricant, wherein the fatty acid salt is stearate. When the environmentally friendly wire drawing lubricant powder is used under the joint action of a certain ratio of each component, the metal wire to be drawn does not need to be pickled during dry drawing, which is environmentally friendly, reduces the process flow during the drawing process, and improves work efficiency. Each component is non-toxic and green. The environmentally friendly wire drawing lubricant powder has good adhesion to the surface of the metal wire and has a better lubricating effect. The environmentally friendly wire drawing lubricant powder is soluble in water and easy to clean. The environmentally friendly wire drawing lubricant powder enables the metal wire to have a higher drawing speed during drawing. The environmentally friendly wire drawing lubricant powder can effectively protect the drawing mold and extend the service life of the mold. Although today's lubricating powder can also have a certain lubricating effect, the raw materials do not use materials such as nano-silica powder and wood cellulose, which causes the lubricating powder to easily clump when encountering some small droplets, which is not conducive to the preservation of the lubricating powder. The overall application effect of the lubricating powder is not good. In order to solve this problem, a metal drawing lubricating powder with a low agglomeration rate is urgently needed. Summary of the invention
[0004] The purpose of the present invention is to solve the problem that although the current lubricating powder can also have a certain lubricating effect, the raw materials do not use materials such as nano-silica powder and wood cellulose, which causes the lubricating powder to easily agglomerate when encountering some small droplets, which is not conducive to the preservation of the lubricating powder and the overall application effect of the lubricating powder is poor. A metal drawing lubricating powder with a low agglomeration rate is proposed.
[0005] In order to achieve the above-mentioned purpose, the present invention adopts the following technical scheme: a metal wire drawing lubricating powder with low agglomeration rate, comprising the following materials: fatty acid salt, sodium nitrite, lubricating filler, additive, vegetable fat, diatom mud, nano-silica powder and wood cellulose.
[0006] As a further description of the above technical solution:
[0007] The weight proportions of the fatty acid salt, sodium nitrite, lubricating filler, additive, vegetable fat, diatom mud, nano-silica powder and wood cellulose are 6-8 parts, 4-6 parts, 3-5 parts, 2-4 parts, 8-10 parts, 5-8 parts, 4-6 parts and 3-7 parts respectively.
[0008] This article also discloses a method for preparing a metal wire drawing lubricating powder with a low agglomeration rate, comprising the following steps:
[0009] S1. Place diatom mud and nano-silica powder in a drying device, provide a certain temperature, and perform rapid drying on the diatom mud and nano-silica powder;
[0010] S2, take out the diatom mud and nano-silica powder and put them into a dispersing device to disperse the mixed materials to ensure that the particle size after dispersion is within a certain value;
[0011] S3, taking vegetable fat and placing it in a mixing device, increasing the temperature of the device, and after the vegetable fat is in a molten state, adding a lubricating filler, increasing the mixing rate of the device, and mixing for a period of time;
[0012] S4, adding wood cellulose into the device, and keeping warm and mixing for a period of time;
[0013] S5, taking fatty acid salt and sodium nitrite and placing them in a grinding device, controlling the grinding device speed, grinding and sieving the mixture;
[0014] S6, putting the sieved mixed material and the granules obtained in S2 into a mixing device at the same time, increasing the mixing rate of the device, and mixing for a period of time;
[0015] S7, finally add auxiliary agent into the mixing device, lower the reaction temperature and maintain it for a period of time;
[0016] S8, taking out the mixed material and placing it in a drying device to quickly dry the mixed material;
[0017] S9. Collect and store the finished products.
[0018] As a further description of the above technical solution:
[0019] In S1, diatom mud and nano-silica powder are placed in a drying device, and a temperature of 70-80° C. is provided to perform a rapid drying treatment on the diatom mud and nano-silica powder.
[0020] As a further description of the above technical solution:
[0021] In S2, the diatom mud and nano-silica powder are taken out and placed in a dispersing device to disperse the mixed materials to ensure that the particle size after dispersion is 5-8 mm.
[0022] As a further description of the above technical solution:
[0023] In S3, vegetable fat is placed in a mixing device, the temperature of the device is increased to 180-200° C., and after the vegetable fat is in a molten state, a lubricating filler is added therein, and the mixing speed of the device is increased to 110-130 r / min, and mixing is performed for a period of time.
[0024] As a further description of the above technical solution:
[0025] In S4, wood cellulose is added into the device and mixed at a temperature of 10-15 minutes.
[0026] As a further description of the above technical solution:
[0027] In S5, fatty acid salt and sodium nitrite are placed in a grinding device, the grinding device speed is controlled to 40-50 r / min, and the mixed material is ground and passed through a 120-140 mesh sieve.
[0028] As a further description of the above technical solution:
[0029] In S6, the sieved mixed material and the granules obtained in S2 are simultaneously put into a mixing device, the mixing speed of the device is increased to 140-160 r / min, and mixed for a period of time.
[0030] As a further description of the above technical solution:
[0031] In the S7, the auxiliary agent is finally added into the mixing device, the reaction temperature is lowered to 110-130°C, and maintained for a period of time. In the S8, the mixed material is taken out and placed in a drying device, and a temperature of 80-90°C is provided to quickly dry the mixed material. During the drying process, the mixed material is continuously turned over by a turning plate.
[0032] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0033] The lubricating powder uses nano-silica powder and wood cellulose in the raw materials. The wood cellulose is insoluble in water, weak acid and alkaline solutions, has high chemical stability, and can maintain the original physical and chemical properties in a variety of environments. Therefore, even if some small amount of droplets in the external environment are mixed in the lubricating powder, it is not easy to cause large-scale agglomeration. It has good moisture-proof effect and is easy to store. At the same time, diatom mud, fatty acid salt, sodium nitrite and the like are also used in the raw materials. These raw materials can effectively improve the granularity of the lubricating powder, so that the lubricating powder has a higher application effect in actual use. At the same time, during the preparation, the mixed material is broken up and ground, which can effectively improve the mixing effect of the powder material, and can also improve the fineness of the powder during the final drying, thereby improving the product quality. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 The present invention is a flow chart of a method for preparing a metal wire drawing lubricating powder with low agglomeration rate. DETAILED DESCRIPTION
[0035] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] Example 1
[0037] See also Figure 1 The present invention provides a technical solution: a metal wire drawing lubricating powder with a low agglomeration rate, comprising the following materials: fatty acid salt, sodium nitrite, lubricating filler, additive, vegetable fat, diatom mud, nano-silica powder and wood cellulose, with the weight proportions being 6-8 parts, 4-6 parts, 3-5 parts, 2-4 parts, 8-10 parts, 5-8 parts, 4-6 parts and 3-7 parts respectively.
[0038] This article also discloses a method for preparing a metal wire drawing lubricating powder with a low agglomeration rate, comprising the following steps:
[0039] S1. Place diatom mud and nano-silica powder in a drying device, provide a temperature of 70°C, and perform rapid drying on the diatom mud and nano-silica powder;
[0040] S2. Take out the diatom mud and nano-silica powder and put them into a dispersing device to disperse the mixed materials to ensure that the particle size after dispersion is 5 mm;
[0041] S3, put the vegetable fat into the mixing device, increase the temperature of the device to 180°C, add lubricating filler into the device after the vegetable fat is in a molten state, increase the mixing speed of the device to 110r / min, and mix for a period of time;
[0042] S4, adding wood cellulose into the device, and mixing at a temperature of 10 minutes;
[0043] S5, taking fatty acid salt and sodium nitrite and placing them in a grinding device, controlling the grinding device speed to 40r / min, grinding the mixture and passing it through a 120-mesh sieve;
[0044] S6, putting the sieved mixed material and the granules obtained in S2 into a mixing device at the same time, increasing the mixing speed of the device to 140 r / min, and mixing for a period of time;
[0045] S7. Finally, add the auxiliary agent into the mixing device, lower the reaction temperature to 110°C, and maintain it for a period of time;
[0046] S8, taking out the mixed material and placing it in a drying device, providing a temperature of 80°C for rapid drying of the mixed material, and using a turning plate to continuously turn the mixed material during the drying process;
[0047] S9. Collect and store the finished products.
[0048] In this embodiment, the lubricating powder uses nano-silica powder and wood cellulose in the raw materials. The wood cellulose is insoluble in water, weak acid and alkaline solutions, and has high chemical stability. It can maintain the original physical and chemical properties in a variety of environments. Therefore, even if some small amount of droplets in the external environment are mixed in the lubricating powder, it is not easy to cause large-scale agglomeration. It has good moisture-proof effect and is easy to store.
[0049] Example 2
[0050] See also Figure 1 The present invention provides a technical solution: a metal wire drawing lubricating powder with a low agglomeration rate, comprising the following materials: fatty acid salt, sodium nitrite, lubricating filler, additive, vegetable fat, diatom mud, nano-silica powder and wood cellulose, with the weight proportions being 6-8 parts, 4-6 parts, 3-5 parts, 2-4 parts, 8-10 parts, 5-8 parts, 4-6 parts and 3-7 parts respectively.
[0051] This article also discloses a method for preparing a metal wire drawing lubricating powder with a low agglomeration rate, comprising the following steps:
[0052] S1. Place diatom mud and nano-silica powder in a drying device, provide a temperature of 75°C, and perform rapid drying on the diatom mud and nano-silica powder;
[0053] S2, take out the diatom mud and nano-silica powder and put them into a dispersing device, and disperse the mixed materials to ensure that the particle size after dispersion is 6mm;
[0054] S3, put the vegetable fat into the mixing device, increase the temperature of the device to 190°C, add lubricating filler into the device after the vegetable fat is in a molten state, increase the mixing speed of the device to 120r / min, and mix for a period of time;
[0055] S4, adding wood cellulose into the device, and mixing it for 12 minutes;
[0056] S5, taking fatty acid salt and sodium nitrite and placing them in a grinding device, controlling the grinding device speed to 45r / min, grinding the mixture and passing it through a 130-mesh sieve;
[0057] S6, putting the sieved mixed material and the granules obtained in S2 into a mixing device at the same time, increasing the mixing speed of the device to 150r / min, and mixing for a period of time;
[0058] S7. Finally, add the auxiliary agent into the mixing device, lower the reaction temperature to 120°C, and maintain it for a period of time;
[0059] S8, taking out the mixed material and placing it in a drying device, providing a temperature of 85°C for rapid drying of the mixed material, and using a turning plate to continuously turn the mixed material during the drying process;
[0060] S9. Collect and store the finished products.
[0061] In this embodiment, diatom mud, fatty acid salts, sodium nitrite, etc. are also used in the raw materials. These raw materials can effectively improve the granularity of the lubricating powder, so that the lubricating powder has a higher application effect in actual use.
[0062] Example 3
[0063] See also Figure 1 The present invention provides a technical solution: a metal wire drawing lubricating powder with a low agglomeration rate, comprising the following materials: fatty acid salt, sodium nitrite, lubricating filler, additive, vegetable fat, diatom mud, nano-silica powder and wood cellulose, with the weight proportions being 6-8 parts, 4-6 parts, 3-5 parts, 2-4 parts, 8-10 parts, 5-8 parts, 4-6 parts and 3-7 parts respectively.
[0064] This article also discloses a method for preparing a metal wire drawing lubricating powder with a low agglomeration rate, comprising the following steps:
[0065] S1. Place diatom mud and nano-silica powder in a drying device, provide a temperature of 80°C, and perform rapid drying on the diatom mud and nano-silica powder;
[0066] S2. Take out the diatom mud and nano-silica powder and put them into a dispersing device to disperse the mixed materials to ensure that the particle size after dispersion is 8 mm;
[0067] S3, put the vegetable fat in a mixing device, increase the temperature of the device to 200°C, add lubricating filler into the device after the vegetable fat is in a molten state, increase the mixing speed of the device to 130r / min, and mix for a period of time;
[0068] S4, adding wood cellulose into the device, and mixing it for 15 minutes;
[0069] S5, taking fatty acid salt and sodium nitrite and placing them in a grinding device, controlling the grinding device speed to 50r / min, grinding the mixture and passing it through a 140-mesh sieve;
[0070] S6, putting the sieved mixed material and the granules obtained in S2 into a mixing device at the same time, increasing the mixing speed of the device to 160r / min, and mixing for a period of time;
[0071] S7. Finally, add the auxiliary agent into the mixing device, lower the reaction temperature to 130°C, and maintain it for a period of time;
[0072] S8, taking out the mixed material and placing it in a drying device, providing a temperature of 90° C. to quickly dry the mixed material, and using a turning plate to continuously turn the mixed material during the drying process;
[0073] S9. Collect and store the finished products.
[0074] In this embodiment, during the preparation, the mixed materials are broken up and ground, which can effectively improve the mixing effect of the powder materials, and can also improve the fineness of the powder during the final drying, thereby improving the product quality.
[0075] Example 4
[0076] See also Figure 1 The present invention provides a technical solution: a metal wire drawing lubricating powder with a low agglomeration rate, comprising the following materials: fatty acid salt, sodium nitrite, lubricating filler, additive, vegetable fat, diatom mud, nano-silica powder and wood cellulose, with the weight proportions being 6-8 parts, 4-6 parts, 3-5 parts, 2-4 parts, 8-10 parts, 5-8 parts, 4-6 parts and 3-7 parts respectively.
[0077] This article also discloses a method for preparing a metal wire drawing lubricating powder with a low agglomeration rate, comprising the following steps:
[0078] S1. Place diatom mud and nano-silica powder in a drying device, provide a temperature of 80°C, and perform rapid drying on the diatom mud and nano-silica powder;
[0079] S2. Take out the diatom mud and nano-silica powder and put them into a dispersing device to disperse the mixed materials to ensure that the particle size after dispersion is 8 mm;
[0080] S3, put the vegetable fat into the mixing device, increase the temperature of the device to 180°C, add lubricating filler into the device after the vegetable fat is in a molten state, increase the mixing speed of the device to 130r / min, and mix for a period of time;
[0081] S4, adding wood cellulose into the device, and keeping warm and mixing for 13 minutes;
[0082] S5, taking fatty acid salt and sodium nitrite and placing them in a grinding device, controlling the grinding device speed to 50r / min, grinding the mixture and passing it through a 140-mesh sieve;
[0083] S6, putting the sieved mixed material and the granules obtained in S2 into a mixing device at the same time, increasing the mixing speed of the device to 160r / min, and mixing for a period of time;
[0084] S7. Finally, add the auxiliary agent into the mixing device, lower the reaction temperature to 120°C, and maintain it for a period of time;
[0085] S8, taking out the mixed material and placing it in a drying device, providing a temperature of 90° C. to quickly dry the mixed material, and using a turning plate to continuously turn the mixed material during the drying process;
[0086] S9. Collect and store the finished products.
[0087] In this embodiment, the lubricating powder uses nano-silica powder and wood cellulose in the raw materials. Wood cellulose is insoluble in water, weak acid and alkaline solutions, has high chemical stability, and can maintain the original physical and chemical properties under various environments. Therefore, even if some small amount of droplets in the external environment are mixed in the lubricating powder, it is not easy to cause large-scale agglomeration. It has good moisture-proof effect and is easy to preserve. At the same time, diatom mud, fatty acid salts, sodium nitrite, etc. are also used in the raw materials. These raw materials can effectively improve the granularity of the lubricating powder, so that the lubricating powder has a higher application effect in actual use. At the same time, during the preparation, the mixed material is broken up and ground, which can effectively improve the mixing effect of the powder material, and can also improve the fineness of the powder during the final drying to improve the product quality.
[0088] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A metal wire drawing lubricating powder with low agglomeration rate, characterized in that: The following materials are included: fatty acid salts, sodium nitrite, lubricating fillers, additives, vegetable fats, diatom mud, nano-silica powder and wood cellulose.
2. The metal wire drawing lubricating powder with low agglomeration rate according to claim 1, characterized in that: The weight proportions of the fatty acid salt, sodium nitrite, lubricating filler, additive, vegetable fat, diatom mud, nano-silica powder and wood cellulose are 6-8 parts, 4-6 parts, 3-5 parts, 2-4 parts, 8-10 parts, 5-8 parts, 4-6 parts and 3-7 parts respectively.
3. A method for preparing a metal wire drawing lubricating powder with a low agglomeration rate, characterized in that: The steps include: S1. Place diatom mud and nano-silica powder in a drying device, provide a certain temperature, and perform rapid drying on the diatom mud and nano-silica powder; S2, take out the diatom mud and nano-silica powder and put them into a dispersing device to disperse the mixed materials to ensure that the particle size after dispersion is within a certain value; S3, taking vegetable fat and placing it in a mixing device, increasing the temperature of the device, and after the vegetable fat is in a molten state, adding a lubricating filler, increasing the mixing rate of the device, and mixing for a period of time; S4, adding wood cellulose into the device, and keeping warm and mixing for a period of time; S5, taking fatty acid salt and sodium nitrite and placing them in a grinding device, controlling the grinding device speed, grinding and sieving the mixture; S6, putting the sieved mixed material and the granules obtained in S2 into a mixing device at the same time, increasing the mixing rate of the device, and mixing for a period of time; S7, finally add auxiliary agent into the mixing device, lower the reaction temperature and maintain it for a period of time; S8, taking out the mixed material and placing it in a drying device to quickly dry the mixed material; S9. Collect and store the finished products.
4. The method for preparing a metal wire drawing lubricating powder with low agglomeration rate according to claim 3, characterized in that: In S1, diatom mud and nano-silica powder are placed in a drying device, and a temperature of 70-80° C. is provided to perform a rapid drying treatment on the diatom mud and nano-silica powder.
5. The method for preparing a metal wire drawing lubricating powder with low agglomeration rate according to claim 3, characterized in that: In S2, the diatom mud and nano-silica powder are taken out and placed in a dispersing device to disperse the mixed materials to ensure that the particle size after dispersion is 5-8 mm.
6. The method for preparing a metal wire drawing lubricating powder with low agglomeration rate according to claim 3, characterized in that: In S3, vegetable fat is placed in a mixing device, the temperature of the device is increased to 180-200° C., and after the vegetable fat is in a molten state, a lubricating filler is added therein, and the mixing speed of the device is increased to 110-130 r / min, and mixing is performed for a period of time.
7. The method for preparing a metal wire drawing lubricating powder with low agglomeration rate according to claim 3, characterized in that: In S4, wood cellulose is added into the device and mixed at a temperature of 10-15 minutes.
8. The method for preparing a metal wire drawing lubricating powder with low agglomeration rate according to claim 3, characterized in that: In S5, fatty acid salt and sodium nitrite are placed in a grinding device, the grinding device speed is controlled to 40-50 r / min, the mixed material is ground and passed through a 120-140 mesh sieve.
9. The method for preparing a metal wire drawing lubricating powder with low agglomeration rate according to claim 3, characterized in that: In S6, the sieved mixed material and the granules obtained in S2 are simultaneously put into a mixing device, the mixing speed of the device is increased to 140-160 r / min, and mixed for a period of time.
10. The method for preparing a metal wire drawing lubricating powder with low agglomeration rate according to claim 3, characterized in that: In the S7, the auxiliary agent is finally added into the mixing device, the reaction temperature is lowered to 110-130°C, and maintained for a period of time. In the S8, the mixed material is taken out and placed in a drying device, and a temperature of 80-90°C is provided to quickly dry the mixed material. During the drying process, the mixed material is continuously turned over by a turning plate.