Heat treatment method of crankshaft blank, crankshaft and application of crankshaft
By tempering and tempering the crankshaft blank, the problems of folding marks and quenching defects after forging of the crankshaft blank are solved, which significantly reduces the quenching waste rate and improves the mechanical performance and reliability of the crankshaft.
Patent Information
- Application Number
- CN202410993392.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-23
AI Technical Summary
The crankshaft blank is prone to folding marks and quenching defects after forging, resulting in a high waste rate of quenching and cracking. The existing heat treatment methods cannot effectively solve this problem.
A method including tempering treatment and tempering treatment is adopted: first, the crankshaft blank is tempered, the temperature is raised to 620℃~680℃, the insulation is 2h~3h, and then the temperature is raised to 840℃~860℃ in the quenching furnace, and the insulation is maintained. 80min~100min, cool down to 790℃~810℃, then heat up to 620℃~640℃ in a tempering furnace, and water-cooled treatment is carried out to reduce thermal stress and deformation.
Significantly reduce the quenching ratio of crankshaft blanks, improve the mechanical properties after forging, reduce the quenching waste rate, and improve the quality and reliability of crankshaft.
Smart Images

Figure CN118932161A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal heat treatment technology, and in particular to a heat treatment method for a crankshaft blank, a crankshaft and applications thereof. Background Art
[0002] The crankshaft is one of the important components inside the engine. Its function is to convert the up and down reciprocating motion of the exhaust piston into continuous rotational motion, thereby driving the engine's output shaft and other key components to operate together, and then drive the movement of vehicles such as cars. The crankshaft is crucial to the performance and reliability of the engine, and its quality directly affects the performance and life of the engine. Some crankshaft blanks need to be processed after quenching and tempering. In the early stage of production, due to lack of experience and other reasons, the forged blanks have folds or other defects, which are prone to quenching cracks during the quenching and tempering process. The quenched and cracked crankshaft blanks can only be scrapped. The quenching crack scrap rate sometimes reaches 3% or even higher, which is a high scrap rate and serious losses.
[0003] Therefore, the current heat treatment method of crankshaft blank still needs to be improved. Summary of the invention
[0004] The present invention aims to alleviate or solve at least one of the above-mentioned problems to at least some extent.
[0005] In one aspect of the present invention, the present invention provides a method for heat treatment of a crankshaft blank. In some embodiments of the present invention, the method for heat treatment of a crankshaft blank comprises the following steps: (1) tempering the crankshaft blank: placing the crankshaft blank in a tempering furnace, heating it to 620°C to 680°C, keeping it warm for 2h to 3h, removing the crankshaft blank from the tempering furnace, and air cooling it to room temperature; (2) quenching and tempering the crankshaft blank after tempering: placing the crankshaft blank air-cooled to room temperature in a quenching furnace, heating it to 840°C to 860°C, keeping it warm for 80min to 100min, cooling it to 790°C to 810°C, keeping it warm for 8min to 28min, removing it from the furnace, placing the crankshaft blank in a quenching tank, cooling it to room temperature, placing the crankshaft blank in a tempering furnace, heating it to 620°C to 640°C, keeping it warm for 80min to 120min, removing the crankshaft blank from the tempering furnace, and water cooling it. Therefore, by using the above method to heat treat the crankshaft blank, defects such as creases in the crankshaft blank after forging can be improved, and the quenching crack ratio of the crankshaft blank can be significantly reduced.
[0006] In some embodiments of the present invention, in step (1), the heating time is 20 minutes to 40 minutes, which is beneficial to the uniform distribution of the temperature inside the crankshaft blank, thereby helping to reduce thermal stress and deformation.
[0007] In some embodiments of the present invention, in step (2), the time taken to raise the temperature to 840°C to 860°C is 20 minutes to 40 minutes. This is beneficial to reducing the thermal stress during the quenching and tempering process, making it difficult for the crankshaft blank to produce defects such as deformation and cracks.
[0008] In some embodiments of the present invention, in step (2), after being kept at 840°C to 860°C, the time taken to cool down to 790°C to 810°C is 8 minutes to 28 minutes. Thus, the internal stress of the structure during quenching can be reduced, which is conducive to further reducing the proportion of quenching cracks in the crankshaft blank.
[0009] In some embodiments of the present invention, in step (2), the quenching tank is filled with a quenching agent, and the quenching agent includes a water-based quenching agent.
[0010] In some embodiments of the present invention, in step (2), the crankshaft blank is placed in a tempering furnace and the temperature is raised to 620° C. to 640° C. for 20 min to 40 min. This is beneficial to uniform distribution of the temperature of the crankshaft blank, thereby further reducing internal stress and cracks.
[0011] In some embodiments of the present invention, the material of the crankshaft blank includes at least one of 42CrMo and 40CrNiMo.
[0012] In some embodiments of the present invention, in step (1), the crankshaft blank is tempered in a mesh-belt tempering furnace; and / or, in step (2), the quenching furnace is a mesh-belt quenching furnace.
[0013] In another aspect of the present invention, the present invention provides a crankshaft. In some embodiments of the present invention, the crankshaft is obtained by heat treating a crankshaft blank using the aforementioned heat treatment method, and then machining the crankshaft blank after the heat treatment. As a result, the crankshaft has excellent mechanical properties and has no obvious defects such as cracks.
[0014] In another aspect of the present invention, the present invention proposes the application of the above crankshaft in a vehicle. The above crankshaft has excellent mechanical properties and does not have obvious defects such as cracks, and is suitable for being used as a crankshaft of an engine or other component in a vehicle. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0016] Figure 1 A physical picture of the crankshaft blank is shown;
[0017] Figure 2A picture showing a crankshaft blank quench cracked scrap;
[0018] Figure 3 A flow chart of a method for heat treating a crankshaft blank according to one embodiment of the present invention is shown;
[0019] Figure 4 A process curve of tempering a crankshaft blank according to an embodiment of the present invention is shown;
[0020] Figure 5 The figure shows a process curve for quenching and tempering a crankshaft blank according to one embodiment of the present invention. DETAILED DESCRIPTION
[0021] The embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.
[0022] The actual picture of the crankshaft blank can be referenced Figure 1 As mentioned above, the crankshaft blank after forging may have folds or other defects (such as stress, etc.), which are prone to quenching cracks during the quenching and tempering process. The crankshaft blank with quenching cracks can refer to Figure 2 , you can see, Figure 2 The crankshaft blank in the forging process has cracks and cannot meet the requirements of the crankshaft inside the engine, so it can only be scrapped. In the related art, directly tempering the crankshaft blank after forging, or normalizing the crankshaft blank before tempering, has little effect on improving the cracks. Normalizing treatment may even aggravate the quenching cracking tendency of the crankshaft blank. The quenching cracking ratio of the crankshaft blank after heat treatment is still high.
[0023] In order to at least alleviate or even solve the problem of high quenching cracking rejection rate of crankshaft blank after quenching and tempering to a certain extent, in one aspect of the present invention, the present invention provides a heat treatment method for crankshaft blank. In some embodiments of the present invention, reference is made to Figure 3 The heat treatment method of the crankshaft blank may include the following steps:
[0024] (1) Tempering the crankshaft blank.
[0025] In some embodiments, reference Figure 4, the forged crankshaft blank can be placed in a tempering furnace, heated to 620℃~680℃, and kept warm for 2h~3h, for example, heated to 620℃, 630℃, 640℃, 650℃, 660℃, 670℃ or 680℃, kept warm for 2h, 2.3h, 2.5h, 2.8h or 3h, and then the crankshaft blank is removed from the tempering furnace and air-cooled to room temperature. Before quenching and tempering the crankshaft blank, adding a high-temperature tempering process can reduce the stress of the crankshaft blank after forging, thereby reducing the proportion of quenching cracks in the crankshaft blank after quenching and tempering.
[0026] In some embodiments of the present invention, in step (1), the heating time can be 20 minutes to 40 minutes, for example, the heating time can be 20 minutes, 25 minutes, 30 minutes, 35 minutes or 40 minutes, thereby, the crankshaft blank can be heated from room temperature to 650°C ± 30°C at a suitable heating rate. During the heating process, the temperature inside the crankshaft blank rises evenly and the temperature distribution is uniform, which is beneficial to reducing the stress after forging, thereby helping to further reduce the risk of quenching cracking of the crankshaft blank after quenching and tempering.
[0027] In some embodiments of the present invention, in step (1), the crankshaft blank can be tempered in a mesh belt tempering furnace.
[0028] In some embodiments of the present invention, the material of the crankshaft blank may include at least one of 42CrMo and 40CrNiMo. In some specific embodiments of the present invention, the material of the crankshaft blank may be 42CrMo or 40CrNiMo. In other specific embodiments of the present invention, the material of the crankshaft blank may include 42CrMo and 40CrNiMo. The crankshaft blank of the above-mentioned material is more likely to have creases and other defects after forging, and is also prone to stress that is difficult to release. The quenching cracking scrap rate after treatment by conventional heat treatment methods (directly quenching and tempering after forging, or, normalizing and quenching and tempering in sequence after forging) is high. Through tempering treatment, the stress after forging can be reduced, and defects such as cracks can be improved, which is conducive to reducing the proportion of quenching cracks in the crankshaft blank after quenching and tempering.
[0029] (2) Tempering the crankshaft blank after tempering.
[0030] After the forged crankshaft blank is tempered, the crankshaft blank can be quenched and tempered.
[0031] In some embodiments of the present invention, in step (2), the crankshaft blank air-cooled to room temperature can be placed in a quenching furnace, heated to 840°C to 860°C, and kept warm for 80 min to 100 min. For example, the crankshaft blank can be placed in a quenching furnace, heated to 840°C, 845°C, 850°C, 855°C or 860°C, and kept warm for 80 min, 85 min, 90 min, 95 min or 100 min.
[0032] In some embodiments of the present invention, in step (2), after keeping the temperature at 840°C to 860°C for a period of time, the temperature is lowered to 790°C to 810°C and kept at this temperature for 8 min to 28 min. For example, the temperature can be lowered to 790°C, 795°C, 800°C, 805°C or 810°C and kept at this temperature for 8 min, 10 min, 15 min, 17 min, 20 min, 22 min, 25 min or 28 min.
[0033] In some embodiments of the present invention, in step (2), after being kept at 790°C to 810°C for a period of time, the crankshaft blank is taken out of the furnace, slides into a quenching tank, and is cooled to room temperature. The crankshaft blank is then placed in a tempering furnace, heated to 620°C to 640°C, and kept warm for 80 min to 120 min. For example, the temperature can be raised to 620°C, 625°C, 630°C, 635°C or 640°C in the tempering furnace, and kept warm for 80 min, 90 min, 100 min, 110 min or 120 min. Thereafter, the crankshaft blank is removed from the tempering furnace and water-cooled.
[0034] During the tempering process, the temperature is first kept at 840℃~860℃ for a period of time, and then the temperature is reduced to 790℃~810℃, and kept at 790℃~810℃ for a period of time. By adjusting the tempering process parameters and lowering the quenching temperature, the internal stress of the organization during quenching can be reduced, which is beneficial to further reduce the proportion of quenching cracks in the crankshaft blank after tempering.
[0035] In some embodiments of the present invention, in step (2), the time taken to heat up to 840°C to 860°C may be 20 min to 40 min, for example, the time taken to heat up to 840°C to 860°C may be 20 min, 25 min, 30 min, 35 min or 40 min. Thus, the temperature may be raised at a suitable heating rate to avoid stress in the crankshaft blank due to uneven heating.
[0036] In some embodiments of the present invention, in step (2), after keeping the temperature at 840°C to 860°C, the time used to cool down to 790°C to 810°C can be 8 min to 28 min. For example, the time used to cool down to 790°C to 810°C can be 8 min, 10 min, 15 min, 20 min, 25 min or 28 min.
[0037] In some embodiments of the present invention, in step (2), a quenching agent is contained in the quenching tank, and the quenching agent may include a water-based quenching agent. Thus, the cooling rate of the water-based quenching agent is between that of water and quenching oil, so that the crankshaft blank can be cooled to room temperature at a relatively gentle rate, which is conducive to reducing quenching stress and preventing the crankshaft blank from deforming or cracking. In some specific embodiments of the present invention, the quenching agent in the quenching tank can use a water-based quenching agent produced by Derunbao Company.
[0038] In some embodiments of the present invention, in step (2), the crankshaft blank is placed in a tempering furnace, and the time taken to heat up to 620°C to 640°C can be 20 minutes to 40 minutes. For example, the time taken to heat up from room temperature to 620°C to 640°C can be 20 minutes, 25 minutes, 30 minutes, 35 minutes or 40 minutes. Thus, heating up at a slower heating rate is beneficial to improving the temperature uniformity inside the crankshaft blank, thereby helping to reduce stress.
[0039] In some embodiments of the present invention, in step (2), the quenching furnace may be a mesh belt quenching furnace.
[0040] In some specific embodiments of the present invention, reference Figure 5 The quenching and tempering of the crankshaft blank after tempering treatment may include the following steps: placing the crankshaft blank air-cooled to room temperature into a mesh belt quenching furnace, heating it to 850°C for 0.5 hours, keeping it warm for 1.5 hours, cooling it to 800°C for 0.3 hours, keeping it warm for 0.3 hours, taking it out of the furnace and sliding it into a quenching tank (with quenching agent) to cool to room temperature, then placing the crankshaft blank into a tempering furnace, heating it to 630°C for 0.5 hours, keeping it warm for 2 hours, taking it out of the furnace and cooling it with water, and sliding it into a material box.
[0041] The quenching cracking phenomenon of the crankshaft blank during the quenching and tempering process is mainly due to defects such as stress and cracks after forging. The defects are inevitable, and remedial measures can only be taken in the subsequent heat treatment process to reduce the quenching cracking ratio. For the purpose of remediation, the present invention mainly starts from two aspects: on the one hand, a high-temperature tempering process is added before quenching and tempering to eliminate the stress of the crankshaft blank after forging, thereby reducing the risk of quenching cracking in the subsequent quenching and tempering process; on the other hand, the process parameters of quenching and tempering are adjusted to reduce the quenching temperature in the quenching and tempering process, from the quenching temperature of 840℃~860℃ to 800℃ after a period of insulation, and then insulation for a period of time, thereby reducing the internal stress of the organization during quenching, and further reducing the risk of quenching cracking in the quenching and tempering process.
[0042] In some embodiments of the present invention, after the crankshaft blank is quenched and tempered, the crankshaft blank can be subjected to performance testing and flaw detection. The performance testing may include hardness testing, metallographic analysis testing, and mechanical property testing, etc.; the flaw detection refers to detecting whether there are quenched cracks in the crankshaft blank after quenching and tempering.
[0043] In the present invention, by performing tempering and quenching and tempering on the crankshaft blank after forging, the risk of quenching cracks in the crankshaft blank tempering process can be reduced, the quenching crack scrap rate of the crankshaft blank can be reduced, and the loss can be reduced.
[0044] In another aspect of the present invention, a crankshaft is provided. In some embodiments of the present invention, the crankshaft may be obtained by heat treating a crankshaft blank by the heat treatment method described above, and then machining the crankshaft blank after the heat treatment. Thus, the crankshaft has good mechanical properties and does not have obvious cracks or other defects.
[0045] In some embodiments of the present invention, machining of the crankshaft blank after heat treatment may include trimming (removing excess material generated during the forging process), shaping (adjusting the shape and size of the crankshaft to ensure that it meets the design requirements), fine machining (such as turning, milling, drilling, etc., to ensure the accuracy and size of the crankshaft), etc.
[0046] In another aspect of the present invention, the present invention proposes the application of the above-mentioned crankshaft in a vehicle. In some embodiments of the present invention, the crankshaft can be used as a component inside a vehicle engine to convert the up and down reciprocating motion of the exhaust piston into continuous rotational motion, thereby driving the output shaft of the engine and other key components to operate together, thereby driving the vehicle to travel. In some embodiments of the present invention, the crankshaft can be used as a component of an engine in a fuel vehicle, an electric vehicle, or a hybrid vehicle.
[0047] The present invention will be described below by specific examples, and it will be appreciated by those skilled in the art that the following specific examples are only for illustrative purposes, and do not limit the scope of the present invention in any way. In addition, in the following examples, unless otherwise specified, the materials and equipment used are all commercially available. If in the following examples, specific processing conditions and processing methods are not clearly described, then conditions and methods known in the art can be used to process.
[0048] Example 1
[0049] In Example 1, the crankshaft blank used is the crankshaft blank of BYD 1.5T hybrid passenger car, the material is 42CrMo, the weight of a single piece is 11.8 kg, and the processing quantity is 1000 pieces.
[0050] The crankshaft blank is subjected to high-temperature tempering treatment: the crankshaft blank is placed in a mesh belt tempering furnace, the temperature is raised to 650°C for 0.5 hours, kept at this temperature for 2 hours, and air-cooled to room temperature after being taken out of the furnace.
[0051] The crankshaft blank after tempering treatment is quenched and tempered: the crankshaft blank air-cooled to room temperature is loaded into a mesh belt quenching furnace, the temperature is raised to 850℃ for 0.5 hours, kept warm for 1.5 hours, cooled to 800℃ for 0.3 hours, kept warm for 0.3 hours, taken out of the furnace and slid into the quenching tank (filled with water-based quenching agent produced by Derunbao Company) to cool to room temperature, and then the crankshaft blank is placed in the tempering furnace, the temperature is raised to 630℃ for 0.5 hours, kept warm for 1.5 hours, taken out of the furnace and water-cooled, and slid into the material box.
[0052] Example 2
[0053] In Example 2, the crankshaft blanks used were BYD 1.5T hybrid passenger car crankshaft blanks, with a single piece weight of 11.8 kg and a processing quantity of 1,000 pieces.
[0054] The crankshaft blank is subjected to high-temperature tempering treatment: the crankshaft blank is placed in a mesh belt tempering furnace, the temperature is raised to 620°C for 20 minutes, and the temperature is kept for 2.5 hours. After being taken out of the furnace, it is air-cooled to room temperature.
[0055] The crankshaft blank after tempering treatment is quenched and tempered: the crankshaft blank air-cooled to room temperature is loaded into a mesh belt quenching furnace, the temperature is raised to 850℃ for 0.5 hours, kept warm for 1.5 hours, cooled to 800℃ for 0.3 hours, kept warm for 0.3 hours, taken out of the furnace and slid into the quenching tank (filled with water-based quenching agent produced by Derunbao Company) to cool to room temperature, and then the crankshaft blank is placed in the tempering furnace, the temperature is raised to 630℃ for 0.5 hours, kept warm for 1.5 hours, taken out of the furnace and water-cooled, and slid into the material box.
[0056] Example 3
[0057] In Example 3, the crankshaft blanks used were BYD 1.5T hybrid passenger car crankshaft blanks, with a single piece weight of 11.8 kg and a processing quantity of 1,000 pieces.
[0058] The crankshaft blank is subjected to high-temperature tempering treatment: the crankshaft blank is placed in a mesh belt tempering furnace, the temperature is raised to 680°C for 40 minutes, and it is kept at this temperature for 3 hours. After being taken out of the furnace, it is air-cooled to room temperature.
[0059] The crankshaft blank after tempering treatment is quenched and tempered: the crankshaft blank air-cooled to room temperature is loaded into a mesh belt quenching furnace, the temperature is raised to 850℃ for 0.5 hours, kept warm for 1.5 hours, cooled to 800℃ for 0.3 hours, kept warm for 0.3 hours, taken out of the furnace and slid into the quenching tank (filled with water-based quenching agent produced by Derunbao Company) to cool to room temperature, and then the crankshaft blank is placed in the tempering furnace, the temperature is raised to 630℃ for 0.5 hours, kept warm for 1.5 hours, taken out of the furnace and water-cooled, and slid into the material box.
[0060] Example 4
[0061] In Example 4, the crankshaft blanks used were BYD 1.5T hybrid passenger car crankshaft blanks, with a single piece weight of 11.8 kg and a processing quantity of 1,000 pieces.
[0062] The crankshaft blank is subjected to high-temperature tempering treatment: the crankshaft blank is placed in a mesh belt tempering furnace, the temperature is raised to 650°C for 0.5 hours, kept at this temperature for 2 hours, and air-cooled to room temperature after being taken out of the furnace.
[0063] The crankshaft blank after tempering treatment is quenched and tempered: the crankshaft blank air-cooled to room temperature is loaded into a mesh belt quenching furnace, heated to 840℃ for 20min, kept warm for 100min, cooled to 810℃ for 8min, kept warm for 28min, taken out of the furnace and slid into the quenching tank (filled with water-based quenching agent produced by Derunbao Company) to cool to room temperature, then the crankshaft blank is put into the tempering furnace, heated to 620℃ for 20min, kept warm for 80min, taken out of the furnace and water-cooled, and slid into the material box.
[0064] Example 5
[0065] In Example 5, the crankshaft blank used is the crankshaft blank of BYD 1.5T hybrid passenger car, the weight of a single piece is 11.8 kg, and the processing quantity is 1000 pieces.
[0066] The crankshaft blank is subjected to high-temperature tempering treatment: the crankshaft blank is placed in a mesh belt tempering furnace, the temperature is raised to 650°C for 0.5 hours, kept at this temperature for 2 hours, and air-cooled to room temperature after being taken out of the furnace.
[0067] The crankshaft blank after tempering treatment is quenched and tempered: the crankshaft blank air-cooled to room temperature is loaded into a mesh belt quenching furnace, heated to 860℃ for 40 minutes, kept warm for 80 minutes, cooled to 800℃ for 28 minutes, kept warm for 8 minutes, taken out of the furnace and slid into the quenching tank (filled with water-based quenching agent produced by Derunbao Company) to cool to room temperature, and then the crankshaft blank is placed in the tempering furnace, heated to 640℃ for 40 minutes, kept warm for 100 minutes, taken out of the furnace and water-cooled, and slid into the material box.
[0068] Example 6
[0069] The difference from Example 1 is that the crankshaft blank in Example 6 uses a Hongqi 1.5T passenger car crankshaft blank, and the weight of a single piece is 13 kg. The remaining parameters and steps are the same as those in Example 1.
[0070] Comparative Example 1
[0071] In Comparative Example 1, the crankshaft blank used was the crankshaft blank of BYD 1.5T hybrid passenger car, the weight of a single piece was 11.8 kg, and the processing quantity was 1,000 pieces.
[0072] Normalizing the crankshaft blank: Place the crankshaft blank in a mesh belt normalizing furnace, heat it to 880°C for 0.5 hours, keep it at this temperature for 1.5 hours, and then take it out of the furnace and air cool it to room temperature.
[0073] Temper the crankshaft blank after normalizing: place the crankshaft blank after normalizing in a mesh belt quenching furnace, heat it to 850℃ for 0.5 hours, keep it warm for 1.5 hours, take it out of the furnace and slide it into a quenching tank (filled with a water-based quenching agent produced by Derunbao Company) to cool to room temperature, place the crankshaft blank cooled to room temperature in a tempering furnace, heat it to 630℃ for 0.5 hours, keep it warm for 1.5 hours, take it out of the furnace and cool it with water, and slide it into the material box.
[0074] Comparative Example 2
[0075] Different from Comparative Example 1, the crankshaft blank is not subjected to normalizing treatment, but directly subjected to quenching and tempering. The remaining parameters and steps are the same as those of Comparative Example 1.
[0076] Comparative Example 3
[0077] Different from Comparative Example 1, the crankshaft blank in Comparative Example 3 uses a Hongqi 1.5T passenger car crankshaft blank, and the weight of a single piece is 13 kg. The remaining parameters and steps are the same as those in Comparative Example 1.
[0078] The crankshaft blanks after heat treatment in each embodiment and comparative example were inspected for quench cracks.
[0079] In Comparative Examples 1 and 3, conventional normalizing plus quenching and tempering treatment methods were used to heat treat the crankshaft blanks, and the quenching cracking ratio of the crankshaft blanks was 3% or more. In Comparative Example 2, only conventional quenching and tempering treatment methods were used to heat treat the crankshaft blanks, and the quenching cracking ratio of the crankshaft blanks was 3% or more. By comparison, it was found that the quenching cracking ratio of the sample in Comparative Example 2 was equivalent to the quenching cracking ratio of the sample in Comparative Example 1. It can be seen that conventional normalizing treatment of the crankshaft blank before quenching and tempering treatment cannot effectively reduce the quenching cracking ratio of the crankshaft blank after quenching and tempering.
[0080] The quenching cracking ratio of the crankshaft blanks in Examples 1 to 6 after heat treatment is all below 0.5%. By comparison, it can be seen that by using the method proposed in the present invention to first perform high-temperature tempering treatment on the crankshaft blank and then perform tempering treatment, the quenching cracking risk of the crankshaft blank during the tempering treatment can be significantly reduced, and the loss of the crankshaft blank scrapped can be greatly reduced.
[0081] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "some specific embodiments", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment are included in at least one embodiment of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art can combine and combine different embodiments or examples described in this specification and the features of different embodiments or examples without contradiction.
[0082] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for heat treatment of a crankshaft blank, It is characterized in that The following steps are involved: (1) Tempering the crankshaft blank: placing the crankshaft blank in a tempering furnace, heating it to 620° C. to 680° C., keeping it at this temperature for 2 h to 3 h, removing the crankshaft blank from the tempering furnace, and air cooling it to room temperature; (2) Tempering the crankshaft blank after tempering: placing the crankshaft blank air-cooled to room temperature in a quenching furnace, heating it to 840°C-860°C, keeping it warm for 80min-100min, cooling it to 790°C-810°C, keeping it warm for 8min-28min, taking it out of the furnace, placing the crankshaft blank in a quenching tank, cooling it to room temperature, placing the crankshaft blank in a tempering furnace, heating it to 620°C-640°C, keeping it warm for 80min-120min, removing the crankshaft blank from the tempering furnace, and water cooling it.
2. The heat treatment method according to claim 1, It is characterized in that In step (1), the heating time is 20 min to 40 min.
3. The heat treatment method according to claim 1, It is characterized in that In step (2), the time taken to raise the temperature to 840°C to 860°C is 20 min to 40 min.
4. The heat treatment method according to claim 1, It is characterized in that In step (2), after being kept at 840°C to 860°C, the time taken to cool down to 790°C to 810°C is 8 minutes to 28 minutes.
5. The heat treatment method according to claim 1, It is characterized in that In step (2), the quenching tank is filled with a quenching agent, and the quenching agent includes a water-based quenching agent.
6. The heat treatment method according to claim 1, It is characterized in that In step (2), the crankshaft blank is placed in a tempering furnace and the temperature is raised to 620° C. to 640° C. for 20 min to 40 min.
7. The heat treatment method according to any one of claims 1 to 6, It is characterized in that The material of the crankshaft blank includes at least one of 42CrMo and 40CrNiMo.
8. The heat treatment method according to any one of claims 1 to 6, It is characterized in that In step (1), the crankshaft blank is tempered in a mesh belt tempering furnace; And / or, in step (2), the quenching furnace is a mesh belt quenching furnace.
9. A crankshaft, It is characterized in that The crankshaft is obtained by heat-treating a crankshaft blank using the heat treatment method according to any one of claims 1 to 8, and then machining the crankshaft blank after the heat treatment.
10. Use of the crankshaft according to claim 9 in a vehicle.
Citation Information
Patent Citations
Crankshaft thermal refining method
CN104480282A
Manufacturing process of large 14Cr17Ni2 stainless steel forgings
CN106854733A
Hardening and tempering treatment technology for roll
CN107177725A
Production process of steam turbine forge piece
CN109536677A
Three-step heat treatment process for 42CrMo crankshaft forged steel for diesel vehicles
CN110438303A
Cited By
Thermal treatment quenching and tempering furnace
CN120272699A