Cadmium metal reduction recovery method and system

By pretreatment, reduction and smelting and vacuum distillation of cadmium metal, the cadmium metal recycling process is simplified, the work efficiency is improved, resource waste and environmental pollution are avoided, and the complex and low-efficiency of cadmium metal recycling in the existing technology is solved. question.

CN118932189APending Publication Date: 2024-11-12广东长信精密设备有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410995123.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing cadmium metal recycling process is complex, has low work efficiency, and is prone to problems such as "running, catching, dripping, and leaking", resulting in waste of resources and environmental pollution risks.

Method used

Using a series of pretreatment, reduction smelting, insulation treatment and vacuum distillation steps, including drying of cadmium-containing materials, heating the alkali to a molten state with the cadmium-containing materials and reducing agents, insulation treatment and vacuum distillation, through these steps Simplify the process, improve the extraction and purification efficiency of cadmium metals, and avoid resource waste and environmental pollution.

Benefits of technology

It realizes efficient extraction and purification of cadmium metal, simplifies the recycling process, improves work efficiency, avoids the occurrence of problems such as "running, catching, dripping, and leaking", and ensures the smoothness and safety of processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932189A_ABST
    Figure CN118932189A_ABST
Patent Text Reader

Abstract

The invention discloses a cadmium metal reduction and recovery method and system.The cadmium metal reduction and recovery method comprises the following steps that a cadmium-containing material is pretreated so as to dry the cadmium-containing material; first caustic soda flakes are heated to a molten state, the temperature of a molten melt reaches a first preset temperature, the dried cadmium-containing material and a reducing agent are sequentially put into the melt for reduction smelting, and the dried cadmium-containing material and the reducing agent are put into the melt multiple times in batches while the melt is stirred, a coarse cadmium material and alkaline residues are obtained; second caustic soda flakes are heated to a second preset temperature, and the crude cadmium material is introduced for heat preservation; and carrying out vacuum distillation on the coarse cadmium material subjected to heat preservation to obtain a cadmium material and alkaline residues. According to the method, the cadmium metal recovery process is simplified, the machining smoothness is guaranteed, the working efficiency is improved, and in addition, through pretreatment, the problems of running, emitting, dripping, leaking and the like are avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of metal recovery, and in particular to a cadmium metal reduction recovery method and system. Background Art

[0002] Current cadmium reduction and recovery equipment is generally complex, often involving multiple steps and processes. This cumbersome process not only increases worker workload but also significantly limits the efficiency of the overall production system. This is particularly true during the cadmium extraction and recovery process, where insufficiently optimized process flows hinder actual efficiency improvements.

[0003] In addition, existing production equipment and technologies often experience material loss during actual operation, such as "running, bubbling, dripping, and leaking". This not only causes a waste of cadmium metal resources, but may also pose safety hazards to the working environment and increase the risk of environmental pollution. Summary of the Invention

[0004] The technical problem to be solved by the present invention is that the existing cadmium metal recovery process is complicated, has low working efficiency, and is prone to problems such as "running, bubbling, dripping, and leaking".

[0005] In order to solve the above technical problems, the present invention provides a cadmium metal reduction and recovery method, comprising the following steps:

[0006] Pre-treating cadmium-containing materials to dry them;

[0007] heating the first caustic soda sheet until it is molten and the temperature of the melt reaches a first preset temperature, adding the dried cadmium-containing material and the reducing agent into the melt in sequence for reduction smelting, and adding the dried cadmium-containing material and the reducing agent in batches multiple times while stirring the melt to obtain a crude cadmium material and alkali residue;

[0008] heating the second caustic soda sheet to a second preset temperature, introducing the crude cadmium material and maintaining the temperature;

[0009] The crude cadmium material after heat preservation is vacuum distilled to obtain cadmium material and alkali residue.

[0010] Furthermore, heating the first caustic soda sheet to a molten state and the melt temperature after melting reaches a first preset temperature includes:

[0011] The heating temperature of the reduction furnace is set to 490-560°C, and a first caustic soda is added to the reduction furnace for heating, so that the first caustic soda is heated to a molten state and the temperature of the melt after melting reaches a first preset temperature, which is greater than 510°C.

[0012] Furthermore, the dried cadmium-containing material and the reducing agent are sequentially added to the melt for reduction smelting, and the dried cadmium-containing material and the reducing agent are added in batches multiple times while stirring the melt to obtain a crude cadmium material and alkali slag, which includes:

[0013] Adding the dried cadmium-containing material into the melt while stirring the melt, and adding a reducing agent and the cadmium-containing material in sequence after stirring to a preset state until the reducing agent is completely added, wherein the reducing agent is carbon powder or granular coal;

[0014] Keep warm and stir for 2-3 hours to obtain crude cadmium material and alkali residue.

[0015] Further, after stirring to a preset state, the method includes:

[0016] If the cadmium-containing material is cadmium powder, a preset amount of cadmium powder is added, and the stirring state is observed. If powder floats on the surface, the reducing agent is added.

[0017] Furthermore, heating the second caustic soda to a second preset temperature and introducing the crude cadmium material for heat preservation comprises:

[0018] Add the second piece of caustic soda into the holding furnace and raise the temperature to 420-470℃;

[0019] The crude cadmium material is introduced until sodium hydroxide flows out of the liquid outlet pipe, and then the temperature is kept constant.

[0020] Furthermore, the crude cadmium material after heat preservation is subjected to vacuum distillation to obtain cadmium material and alkali residue, including:

[0021] 3.5-5 L / min nitrogen is introduced into the holding furnace, and a vacuum operation is performed to draw the crude cadmium material in the holding furnace into the distillation furnace, and the vacuum is evacuated to a pressure of <50 Pa;

[0022] The crude cadmium material in the distillation furnace is heated to 510-560° C. for rectification to obtain cadmium material and alkali slag.

[0023] Furthermore, heating the crude cadmium material in the distillation furnace and raising the temperature to 510-560° C. for distillation further comprises:

[0024] When 1 / 3-1 / 4 of the crude cadmium material remains in the distillation furnace, the crude cadmium material is extracted again and put into the distillation furnace for distillation, and the distillation tail material is emptied every 32-37 times.

[0025] Furthermore, the crude cadmium material after insulation is subjected to vacuum distillation to obtain cadmium material and alkali residue, which includes:

[0026] The cooling water system of the cadmium rod machine was turned on, the rod pulling speed was set to 1-12 mm / min, the shearing distance was set to 200 mm, the cadmium material was transported to the cadmium rod machine, and the cadmium rod was started to be pulled, and then the cadmium rod was sheared.

[0027] Furthermore, pre-treating the cadmium-containing material to dry the cadmium-containing material includes:

[0028] Put the cadmium-containing materials into the drying kiln, set the calcination temperature to 480-570℃, and keep the temperature for 4.5-5.5 hours after the temperature in the kiln reaches 510℃.

[0029] The present invention also provides a cadmium metal reduction system, which uses the cadmium metal reduction and recovery method described above to recover cadmium metal. The cadmium metal reduction system includes: a reduction furnace, an alkali slag flaker, a cadmium discharge chute assembly, an alkali slag discharge chute assembly, a holding furnace, a crude cadmium material feed pipe, a distillation furnace, a refined cadmium discharge pipe, a vacuum assembly, a rod casting machine, a dust removal assembly, and a drying kiln.

[0030] The reduction furnace and the alkali slag flaker are connected through the alkali slag discharge chute assembly, and the reduction furnace and the holding furnace are connected through the cadmium discharge chute assembly, the holding furnace and the distillation furnace are connected through the crude cadmium material feed pipe, the distillation furnace and the rod casting machine are connected through the refined cadmium discharge pipe, and the vacuum assembly is connected to the distillation furnace, and the dust removal assembly is connected to the reduction furnace, the alkali slag flaker, the holding furnace and the rod casting machine.

[0031] Compared with the prior art, the cadmium metal reduction and recovery method and system according to the embodiment of the present invention have the following beneficial effects:

[0032] The embodiment of the present invention performs a series of processing steps such as pretreatment, reduction smelting, insulation treatment and vacuum distillation on the cadmium-containing material, thereby achieving efficient extraction and purification of valuable cadmium metal in the cadmium-containing material, simplifying the cadmium metal recovery process, ensuring the smoothness of processing, and improving work efficiency. In addition, through pretreatment, the occurrence of problems such as "escape, bubbling, dripping, and leakage" is avoided. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 is a front view of a cadmium metal reduction system provided by an embodiment of the present invention;

[0034] Figure 2 is a rear view of a cadmium metal reduction system provided by an embodiment of the present invention;

[0035] Figure 3 is a top view of a cadmium metal reduction system provided by an embodiment of the present invention;

[0036] Figure 4is a flow chart of a cadmium metal reduction and recovery method provided by an embodiment of the present invention;

[0037] In the figure, 1. Reduction furnace; 2. Alkali slag flaker; 3. Cadmium discharge chute assembly; 4. Alkali slag discharge chute assembly; 5. Holding furnace; 6. Crude cadmium material feed pipe; 7. Distillation furnace; 8. Refined cadmium discharge pipe; 9. Vacuum assembly; 901. First-stage vacuum pipe; 902. Second-stage vacuum pipe; 903. Vacuum gas-solid separation tank; 904. Rotary vane vacuum pump; 10. Rod casting machine; 11. Dust removal assembly; 1101. Dust collection pipe network assembly; 1102. Dust collection equipment installation Platform; 1103, fluidizing tower; 1104, cyclone dust collector; 1105, sintering plate dust collector; 1106, dust collecting induced draft fan; 1107, chimney; 1108, adsorbent powder adding device; 12, drying kiln; 13, fixed column cantilever crane; 14, reduction furnace operating platform; 15, holding furnace slag scooping platform; 16, rod casting machine charging furnace; 17, rod casting machine charging furnace platform; 18, steel plate; 19, weighing module; 20, asbestos cement board; 21, closed water cooling tower. DETAILED DESCRIPTION

[0038] The following embodiments of the present invention are described in further detail with reference to the accompanying drawings and examples. The following examples are used to illustrate the present invention but are not intended to limit the scope of the present invention.

[0039] like Figures 1 to 3 As shown, the present invention provides a cadmium metal reduction system, comprising: a reduction furnace 1, an alkali slag flaker 2, a cadmium discharge chute assembly 3, an alkali slag discharge chute assembly 4, a holding furnace 5, a crude cadmium material feed pipe 6, a distillation furnace 7, a refined cadmium discharge pipe 8, a vacuum assembly 9, a rod casting machine 10, a dust removal assembly 11 and a drying kiln 12; the reduction furnace 1 and the alkali slag flaker 2 are connected via the alkali slag discharge chute assembly 4, and the reduction furnace 1 and the holding furnace 5 are connected via the cadmium discharge chute assembly 3, the holding furnace 5 and the distillation furnace 7 are connected via the crude cadmium material feed pipe 6, the distillation furnace 7 and the rod casting machine 10 are connected via the refined cadmium discharge pipe 8, and the vacuum assembly 9 is connected to the distillation furnace 7, and the dust removal assembly 11 is connected to the reduction furnace 1, the alkali slag flaker 2, the holding furnace 5 and the rod casting machine 10.

[0040] Based on the above structure, the reduction furnace 1 of this embodiment is used to reduce cadmium-containing compounds or waste materials (i.e., cadmium-containing materials) to elemental cadmium or crude cadmium form (i.e., crude cadmium materials). The reduction furnace 1 transfers the crude cadmium materials obtained by reduction from the reduction furnace 1 to the holding furnace 5 via the cadmium discharge chute assembly 3 for temporary storage and maintenance of the temperature of the crude cadmium materials, thereby ensuring the continuity of the subsequent purification process. In addition, the reduction furnace 1 discharges the alkali slag produced during the reduction process from the reduction furnace 1 via the alkali slag discharge chute assembly 4 and transports it to the alkali slag flaker 2 for processing the alkali slag produced during the reduction process and solidifying it into a solid form that is convenient for storage and processing. Subsequently, the holding furnace 5 is connected to the distillation furnace 7 via the crude cadmium material feed pipe 6 to feed the crude cadmium material into the distillation furnace 7 for further purification. The purified refined cadmium (i.e., cadmium material) enters the rod casting machine 10 for molding through the refined cadmium discharge pipe 8.

[0041] In actual application, the entire production line is equipped with a dust removal system connected to various equipment to collect and treat dust and other harmful gases generated during the production process to ensure compliance with environmental protection standards and worker safety and health requirements. The drying kiln 12 is used to dry cadmium-containing materials to reduce the occurrence of "running, bubbling, dripping or leaking" and other phenomena.

[0042] In some embodiments, a fixed column jib crane 13 and a reduction furnace operating platform 14 are also included. The reduction furnace 1 is mounted on the reduction furnace operating platform 14. The fixed column jib crane 13 is used to transfer the cadmium byproduct into the reduction furnace 1, thereby significantly reducing the risk of manual feeding. The fixed column jib crane 13 is a 2-ton fixed column jib crane.

[0043] A slag removal platform 15 is located next to the holding furnace 5 to facilitate the removal of alkali slag. The rod casting machine 10 and the distillation furnace 7 are connected via a rod casting machine charging furnace 16, with a rod casting machine charging furnace platform 17 located next to the charging furnace 16 to facilitate operations. Furthermore, a steel plate 18, a weighing module 19, and an asbestos cement board 20 are located below the distillation furnace 7. The asbestos cement board 20 provides a mounting platform for the distillation furnace 7. The weighing module 19 is connected to the distillation furnace 7 via the steel plate 18 to monitor the weight of the distillation furnace 7 in real time, facilitating the determination of the remaining material within the distillation furnace 7.

[0044] In some embodiments, the vacuum assembly 9 includes a first-level vacuum tube 901, a second-level vacuum tube 902, a vacuum air-solid separation tank 903 and a rotary vane vacuum pump 904. The refined cadmium discharge pipe 8 and the second-level vacuum tube 902 are connected through the first-level vacuum tube 901, and the end of the second-level vacuum tube 902 away from the first-level vacuum tube 901 is connected to the vacuum air-solid separation tank 903, and the rotary vane vacuum pump 904 is connected to the vacuum air pipe separation tank.

[0045] During the refined cadmium extraction process, this embodiment extracts gas from the distillation furnace 7 to provide a vacuum environment for cadmium distillation and purification. The vacuum gas-solid separation tank 903 receives the vacuumized mixed gas and performs gas-solid separation there. This effectively intercepts and collects solid particles (which may include cadmium particles or other impurities) in the gas, preventing them from entering the vacuum pump, thereby protecting the vacuum pump from contamination and extending the service life of the equipment. Furthermore, a rotary vane vacuum pump 904 is used to provide power for vacuuming and extract the separated pure gas, further reducing the pressure within the entire distillation system and ensuring that the cadmium metal purification process is carried out stably and efficiently under a high vacuum state.

[0046] The dust collection assembly 11 includes a dust collection pipe network assembly 1101, a dust collection equipment installation platform 1102, a fluidized bed 1103, a cyclone dust collector 1104, a sintered plate dust collector 1105, a dust collection fan 1106, a chimney 1107, an adsorbent powder adding device 1108, and an adsorbent circulation fan; the fluidized bed 1103, the cyclone dust collector 1104 and the sintered plate dust collector 1105 are arranged on the dust collection equipment installation platform 1102, and ... 104 and the sintering plate dust collector 1105 are connected in sequence, and the end of the fluidized tower 1103 away from the cyclone dust collector 1104 is connected to the reduction furnace 1, the alkali slag flake machine 2, the insulation furnace 5 and the rod casting machine 10 through the dust collecting pipe network assembly 1101, and the end of the sintering plate dust collector 1105 away from the cyclone dust collector 1104 is connected to the chimney 1107 through the dust collecting draft fan 1106, and the adsorbent circulation fan and the fluidized tower 1103 are connected through the adsorbent powder adding device 1108.

[0047] The dust collection pipe network assembly 1101 in this embodiment is used to transfer the dust generated by each production link to the fluidized tower 1103. The fluidized tower 1103 uses the fluidization principle to make the dust fully contact with a certain medium (such as water or gas) to facilitate subsequent dust separation and capture. The cyclone dust collector 1104 is then used to separate the particulate matter in the dust-laden airflow. The sintered plate dust collector 1105 intercepts and captures the dust, and the dust-laden gas is forced to enter and pass through each dust removal device along a predetermined path through the dust collection fan 1106. Finally, the purified gas is discharged into the chimney 1107, and finally, the relatively clean gas after dust removal is discharged into the atmosphere. In addition, the adsorbent powder adding device 1108 replenishes or replaces the adsorbent to the fluidized tower 1103 to maintain a good adsorption effect, and the adsorbent circulation fan promotes the circulation of the adsorbent in the fluidized tower 1103 to ensure that the adsorption reaction is fully carried out.

[0048] In actual use, a closed water cooling tower 21 is also included to provide cooling water for the cadmium rod machine. Furthermore, the drying kiln 12, reduction furnace 1, holding furnace 5, and refined cadmium holding furnace 5 are all equipped with dust collection hoods to prevent dust from being generated. A dust collection pipe network assembly 1101 is also used to collect dust within the dust collection hoods.

[0049] like Figure 4 As shown, the cadmium metal reduction system uses the following cadmium metal reduction recovery method to recover cadmium metal. The cadmium metal reduction recovery method includes the following steps:

[0050] S110, pre-treating the cadmium-containing material to dry the cadmium-containing material;

[0051] This step is the pretreatment stage, which involves drying the cadmium-containing material to remove excess moisture from the material, thereby avoiding problems such as bubbling and leakage caused by the presence of moisture during the reduction smelting process.

[0052] S120, heating the first caustic soda sheet until it is molten and the temperature of the melt reaches a first preset temperature, adding the dried cadmium-containing material and the reducing agent into the melt in sequence for reduction smelting, and adding the dried cadmium-containing material and the reducing agent in batches multiple times while stirring the melt to obtain a crude cadmium material and alkali residue;

[0053] This step is the reduction smelting stage, in which the first piece of caustic soda is heated to the preset requirements to ensure that the reaction conditions are appropriate. While the melt is continuously stirred, the dried cadmium-containing material and the reducing agent are added to the melt in batches for a reduction reaction, so as to reduce the cadmium oxide or other compounds to cadmium element through a chemical reaction at high temperature until all the cadmium-containing materials have completed the reaction, and finally a crude cadmium material (a mixture containing a certain proportion of cadmium metal) and alkali slag (waste after the reaction) are obtained, wherein the first piece of caustic soda is sodium hydroxide.

[0054] S130, heating the second caustic soda to a second preset temperature, introducing the crude cadmium material and keeping it warm;

[0055] This step is the crude cadmium material insulation stage. The crude cadmium material obtained is then heated and contacted with a second sheet of caustic soda heated to a second preset temperature for insulation treatment. This process helps maintain the temperature of the crude cadmium material, ensuring the smoothness of subsequent steps. It also allows the caustic soda to dissolve or react other impurities, thereby effectively separating the cadmium metal. It should be noted that the second sheet of caustic soda in this embodiment is made of the same material as the first sheet of caustic soda.

[0056] S140, vacuum distilling the crude cadmium material after heat preservation to obtain cadmium material and alkaline residue.

[0057] This step is the vacuum distillation purification stage, in which the crude cadmium material after heat preservation is placed in a vacuum environment for distillation. Due to the difference in boiling points between cadmium and other impurities, cadmium can be effectively separated from other components under different vacuum conditions. After vacuum distillation, a higher purity cadmium material is obtained, and the remaining product still containing unreacted alkali and other non-volatile components becomes alkaline slag.

[0058] Based on the above method, the cadmium-containing materials are subjected to a series of processing steps including pretreatment, reduction smelting, insulation treatment and vacuum distillation, thereby achieving efficient extraction and purification of valuable cadmium metal in the cadmium-containing materials, simplifying the cadmium metal recovery process, ensuring the smoothness of processing, and improving work efficiency. In addition, through pretreatment, the occurrence of problems such as "running, bubbling, dripping, and leaking" is avoided.

[0059] Furthermore, heating the first caustic soda to a molten state and the melt temperature after melting reaches a first preset temperature includes: setting the heating temperature of the reduction furnace 1 to 490-560°C for heating, and adding the first caustic soda into the reduction furnace 1 for heating, so that the first caustic soda is heated to a molten state and the melt temperature after melting reaches a first preset temperature, and the first preset temperature is greater than 510°C.

[0060] In this embodiment, the heating temperature range is set to 490-560°C to melt the sodium hydroxide into a liquid state and ensure that the entire melt is fully fluid and reactive. Furthermore, the first preset temperature is used to ensure that the cadmium-containing material reacts quickly and effectively with the alkaline melt upon contact, and to ensure that the molten first caustic soda has good solubility and reduction capabilities for the cadmium compounds in the cadmium-containing material at this temperature.

[0061] Furthermore, while stirring the melt, the dried cadmium-containing material and the reducing agent are sequentially added into the melt for reduction smelting, and the dried cadmium-containing material and the reducing agent are added in batches multiple times while stirring the melt to obtain a crude cadmium material and alkali slag, which includes:

[0062] S121, adding the dried cadmium-containing material into the melt while stirring the melt, and after stirring to a preset state, sequentially adding a reducing agent and the cadmium-containing material until the reducing agent is completely added, wherein the reducing agent is carbon powder or granular coal;

[0063] In this step, the first sheet of alkali has been heated to a molten state and has reached a suitable preset temperature. At this point, the operator will gradually add the cadmium-containing material that has been pre-dried to the molten alkali solution in batches while continuously stirring the melt. The purpose of stirring is to allow the cadmium-containing material to fully contact and mix with the alkali solution, thereby promoting the uniform progress of the chemical reaction. It should be noted that the cadmium-containing material is not added all at once, but is added in batches, and a reducing agent is added in due time between each batch of cadmium-containing material. Granular coal or carbon powder acts as a reducing agent, which can react chemically with the cadmium compounds in the cadmium-containing material under high temperature conditions to reduce the cadmium element.

[0064] S123, keeping warm and stirring for 2-3 hours to obtain crude cadmium material and alkaline residue.

[0065] In this step, after all reducing agents are added in batches, the entire smelting is kept warm and stirred for about 2 to 3 hours to ensure the progress of the reduction reaction and form crude cadmium material, while other components that fail to participate in the reaction and the reaction products form alkaline slag.

[0066] In this embodiment, crude cadmium material is extracted from the cadmium-containing material in the above manner. At the same time, the remaining components in the waste are immobilized, that is, alkaline slag that is easy to dispose of is formed, which not only realizes the recovery of cadmium resources but also effectively controls the emission of pollutants.

[0067] Furthermore, after stirring to a preset state, the method includes: if the cadmium-containing material is cadmium powder, adding a preset amount of cadmium powder, observing the stirring state, and starting to add a reducing agent if powder floats on the surface.

[0068] During the stirring process, it was found that some cadmium powder was not fully mixed and floated on the surface of the liquid, indicating that it may not be fully wetted or unevenly dispersed. At this time, a reducing agent was added to improve the dispersibility of the cadmium powder in the medium and prevent it from agglomerating or settling. It should be noted that for full reduction, carbon powder was added at a rate of approximately 4 kg / min and stirring was continued.

[0069] Furthermore, heating the second caustic soda to a second preset temperature and introducing the crude cadmium material for heat preservation comprises:

[0070] S131, add a second piece of caustic soda into the holding furnace 5 and raise the temperature to 420-470°C;

[0071] In this step, a second piece of caustic soda is added to the holding furnace 5 for subsequent reaction or adsorption with impurities in the crude cadmium material to improve the purity of cadmium. At the same time, the holding furnace 5 is heated to 420 to 470° C. to ensure that the sodium hydroxide is fully melted and maintains good reaction activity at high temperatures.

[0072] S132. Add crude cadmium material until sodium hydroxide flows out of the liquid outlet pipe, and then keep warm.

[0073] In this step, after the temperature in the holding furnace 5 reaches a preset value, the crude cadmium material obtained from the previous reduction smelting is slowly introduced into the molten sodium hydroxide. When sodium hydroxide begins to flow out of the liquid outlet pipe, the crude cadmium material has now fully come into contact with the molten sodium hydroxide and some impurities have been removed. At this point, the introduction of new crude cadmium material is stopped, and the holding stage is switched to allow the remaining impurities to react with the alkali solution as much as possible, while preventing the loss of cadmium metal.

[0074] Based on the above description, it can be seen that the main function of the insulation stage of this embodiment is to further stabilize the chemical reaction that occurred previously, ensure that the cadmium element in the crude cadmium material is retained in a solid metal state as much as possible, and that impurities are removed to the maximum extent possible, thereby ultimately obtaining a cadmium product with higher purity while ensuring the temperature stability of the crude cadmium material, so as to facilitate the subsequent process and ensure the smoothness of the reaction.

[0075] Furthermore, the crude cadmium material after heat preservation is vacuum distilled to obtain cadmium material and alkali residue including:

[0076] S141, introducing 3.5-5 L / min nitrogen into the holding furnace 5, and performing a vacuum operation to draw the crude cadmium material in the holding furnace 5 into the distillation furnace 7, and evacuate to a pressure of <50 Pa;

[0077] In this step, nitrogen gas is introduced into holding furnace 5 at a rate of 3.5-5 L / min to displace oxygen, preventing oxidation reactions in the high-temperature vacuum environment and protecting the cadmium material from damage. This nitrogen also aids in the material transfer process. Subsequently, a vacuum pump is used to extract the crude cadmium material from holding furnace 5 at a pressure below 50 Pa and introduce it into distillation furnace 7. This vacuuming operation aims to reduce gas resistance during the distillation process, facilitating the evaporation and separation of cadmium and its impurities under low-pressure conditions.

[0078] S142, heating the crude cadmium material in the distillation furnace 7 and raising the temperature to 510-560° C. for distillation to obtain cadmium material and alkaline slag.

[0079] In this step, the crude cadmium material transferred to the distillation furnace 7 is heated to 510-560° C. and subjected to a rectification process to ensure more effective separation of cadmium from other impurities under vacuum conditions to form a cadmium material with higher purity.

[0080] Through the above operations, this embodiment further improves the purity of cadmium, separates cadmium from crude cadmium material by physical distillation, and leaves impurities that cannot be sublimated in the alkaline slag, thereby achieving efficient recovery and purification of cadmium metal.

[0081] Furthermore, heating the crude cadmium material in the distillation furnace 7 to 510-560° C. for distillation further comprises:

[0082] When 1 / 3-1 / 4 of the crude cadmium material remains in the distillation furnace 7, the crude cadmium material is extracted again and put into the distillation furnace 7 for distillation, and the distillation tail material is emptied every 32-37 times.

[0083] During this step, during the cadmium metal distillation process, the operator heats the crude cadmium material placed in the distillation furnace 7 to a temperature between 510 and 560°C to ensure that the cadmium and its impurities can be effectively separated at high temperatures due to their boiling point differences. When the crude cadmium material in the furnace is consumed by distillation to approximately 1 / 3-1 / 4 of the remaining crude cadmium material, new crude cadmium material is pumped into the distillation furnace 7 for a new round of distillation to ensure that there is always enough material in the furnace for continuous distillation operations, thereby improving the efficiency of the equipment.

[0084] In addition, the distillation tailings, that is, the residue that cannot be further sublimated or separated after multiple distillations, are emptied once every 32-37 distillation cycles to regularly clean the difficult-to-volatile impurities that cannot be effectively distilled and accumulated in the distillation furnace 7 to prevent their accumulation from affecting the distillation efficiency and purity of cadmium. At the same time, it is also convenient for the proper handling of the tailings to ensure the continuity and stability of the process.

[0085] Furthermore, the crude cadmium material after heat preservation is subjected to vacuum distillation to obtain cadmium material and alkali residue, which includes:

[0086] Turn on the cooling water system of the cadmium rod machine, set the rod pulling speed to 1-12mm / min, set the shearing distance to 200mm, transport the cadmium material to the cadmium rod machine, start pulling the cadmium rod, and then shear the cadmium rod.

[0087] In this step, the cooling water system is turned on to control the heat generated by the cadmium during the rod drawing process and dissipate it in time, ensuring that the cadmium rod is kept at a suitable temperature during forming to prevent the cadmium from overheating, deformation, or quality damage. In addition, the rod drawing speed is set to 1-12mm / min to avoid excessive speed, which may cause uneven internal structure or cracks in the cadmium rod, while excessive speed affects production efficiency. At the same time, the shear distance is also set to 200mm to ensure that the cadmium rods are of consistent length for subsequent packaging, transportation, and use.

[0088] Furthermore, the cadmium-containing material is pretreated to dry the cadmium-containing material, including: putting the cadmium-containing material into a drying kiln 12, setting the calcination temperature to 480-570° C., and keeping the temperature for 4.5-5.5 hours after the temperature in the kiln reaches 510° C.

[0089] During this process, the drying kiln 12 is set at a calcination temperature range of 480-570°C to ensure rapid evaporation of moisture from the cadmium-containing material, preventing problems such as escaping, bubbling, dripping, and leaking. After the kiln temperature stabilizes at a minimum of 510°C, the hold phase begins, lasting 4.5-5.5 hours. During this phase, the cadmium-containing material is maintained at a high temperature to ensure complete removal of moisture from both the interior and surface of the material, while also preheating the material to facilitate smooth processing in subsequent steps.

[0090] The specific workflow is as follows:

[0091] Turn on the dust collecting fan 1106, start the cyclone dust collector 1104 and the sintering plate dust collector 1105, and collect and treat the waste gas and tail gas generated during the operation of the equipment.

[0092] Pretreatment of cadmium hydroxide and cadmium carbonate: put 1.2-1.6 tons of cadmium hydroxide by-product into the drying kiln 12, set the calcination temperature to 480-570℃, keep it warm for 4.5-5.5 hours after the temperature in the drying kiln 12 reaches 510℃, and then unload all the cadmium oxide into the barrel. After all the cadmium oxide is unloaded, it can be fed again.

[0093] Adding alkali and melt: Add sodium hydroxide to reduction furnace 1, set the temperature to 490-560°C, and start heating. Once all the sodium hydroxide in the furnace has melted and the melt temperature is >510°C, start stirring. Add cadmium material to reduction furnace 1. If the cadmium material is cadmium powder, add 55-110 kg. Observe the stirring status. If powder floats to the surface, start adding carbon powder. Add 15-20 kg of carbon powder to reduction furnace 1. Then, continue adding cadmium powder or cadmium oxide. Add carbon powder to reduction furnace 1 at a rate of 4-6 kg / min. After all the carbon powder has been added, continue to maintain the temperature and stir for 2-3 hours. Add 35-55 kg of sodium hydroxide to holding furnace 5 and raise the temperature to 420-470°C. Open the conical valve on the cadmium discharge pipe of reduction furnace 1 to discharge the reduced cadmium material into holding furnace 5. Stop discharging when sodium hydroxide begins to flow from the liquid outlet pipe of reduction furnace 1 and close the conical valve. The alkali liquid outlet pipe of the reduction furnace 1 is opened, and the alkali liquid is discharged to the alkali slag flake machine through the alkali slag chute assembly 4 for flake making. The sodium hydroxide in the holding furnace 5 is replaced every five days, and the alkali slag is discharged and put into the reduction furnace 1 for use.

[0094] Distillation: Turn on the heating systems of the distillation furnace 7 and the rod casting machine feed furnace 16, raise the temperature to 420-470°C, turn on the vacuum pump, evacuate to a pressure of <50Pa, and introduce nitrogen into the rod casting machine feed furnace 16 at a rate of 3.5-5L / min. Pump the cadmium liquid in the 1# holding furnace 5 into the distillation furnace 7, raise the temperature to 510-560°C for distillation. When 1 / 3-1 / 4 of the material in the distillation remains, pump the cadmium liquid into the distillation furnace 7 again for distillation. The distillation tailings are emptied every 32-37 times. The distilled cadmium material flows into the rod casting machine feed furnace 16.

[0095] Casting: Turn on the cooling water system of the cadmium rod machine, set the rod pulling speed to 1-12mm / min, set the shearing distance to 200mm, open the taper valve of the discharge pipe of the rod casting furnace 16, and start pulling the cadmium rods. Collect the sheared cadmium rods and place them in the material box for packaging.

[0096] In summary, the embodiments of the present invention provide a cadmium metal reduction and recovery method and system with a simple structure, ease of operation, and high flexibility. This method can reduce labor intensity, improve processing efficiency, provide more flexible and convenient operation, and ensure safe production. Furthermore, the above method and system do not require excessive manual operation, thus avoiding the waste of raw materials and redundant labor caused by excessive manual operation.

[0097] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and substitutions can be made without departing from the technical principles of the present invention. These improvements and substitutions should also be regarded as the scope of protection of the present invention.

Claims

1. A cadmium metal reduction and recovery method, characterized in that: The steps include: Pre-treating cadmium-containing materials to dry the cadmium-containing materials; The first alkali sheet is heated to a molten state and the temperature of the melt after melting reaches a first preset temperature, and the dried cadmium-containing material and the reducing agent are sequentially added into the melt for reduction smelting, and the dried cadmium-containing material and the reducing agent are added in batches for multiple times while stirring the melt, so as to obtain a crude cadmium material and alkali slag; heating the second caustic soda sheet to a second preset temperature, and introducing the crude cadmium material to keep the temperature; The crude cadmium material after heat preservation is subjected to vacuum distillation to obtain cadmium material and alkaline slag.

2. The cadmium metal reduction and recovery method according to claim 1, characterized in that: Heating the first alkali sheet to a molten state and the melt temperature after melting reaches a first preset temperature comprises: The heating temperature of the reduction furnace is set to 490-560°C, and a first sheet of caustic soda is added into the reduction furnace for heating, so that the first sheet of caustic soda is heated to a molten state and the temperature of the melt after melting reaches a first preset temperature, and the first preset temperature is greater than 510°C.

3. The cadmium metal reduction and recovery method according to claim 1, characterized in that: The process of sequentially adding the dried cadmium-containing material and the reducing agent into the melt for reduction smelting, and adding the dried cadmium-containing material and the reducing agent in batches for multiple times while stirring the melt to obtain a crude cadmium material and alkali slag comprises: Adding the dried cadmium-containing material into the melt while stirring the melt, and after stirring to a preset state, adding a reducing agent and the cadmium-containing material in sequence until the reducing agent is completely added, wherein the reducing agent is carbon powder or granular coal; Keep warm and stir for 2-3 hours to obtain crude cadmium material and alkaline slag.

4. The cadmium metal reduction and recovery method according to claim 3, characterized in that: After stirring to the preset state, it includes: If the cadmium-containing material is cadmium powder, after adding a preset amount of cadmium powder, observe the stirring state, and if there is powder floating on the surface, start adding the reducing agent.

5. The cadmium metal reduction and recovery method according to claim 1, characterized in that: The second caustic soda sheet is heated to a second preset temperature, and the crude cadmium material is introduced for heat preservation, comprising: Add the second piece of caustic soda into the holding furnace and raise the temperature to 420-470℃; The crude cadmium material is introduced until sodium hydroxide flows out of the liquid outlet pipe, and then the temperature is kept high.

6. The cadmium metal reduction and recovery method according to claim 1, characterized in that: The crude cadmium material after heat preservation is subjected to vacuum distillation to obtain cadmium material and alkali slag including: 3.5-5 L / min of nitrogen is introduced into the holding furnace, and a vacuum operation is performed to draw the crude cadmium material in the holding furnace into the distillation furnace, and the vacuum is evacuated to a pressure of <50 Pa; The crude cadmium material in the distillation furnace is heated to 510-560° C. for distillation to obtain cadmium material and alkali slag.

7. The cadmium metal reduction and recovery method according to claim 6, characterized in that: The step of heating the crude cadmium material in the distillation furnace to 510-560° C. for distillation further comprises: When 1 / 3-1 / 4 of the crude cadmium material remains in the distillation furnace, the crude cadmium material is again extracted and put into the distillation furnace for distillation, and the distillation tail material is emptied every 32-37 times.

8. The cadmium metal reduction and recovery method according to claim 1, characterized in that: The crude cadmium material after heat preservation is subjected to vacuum distillation to obtain cadmium material and alkali slag, which includes: The cooling water system of the cadmium rod machine is turned on, the rod pulling speed is set to 1-12 mm / min, the shearing distance is set to 200 mm, the cadmium material is transported to the cadmium rod machine, and the cadmium rod is started to be pulled, and then the cadmium rod is sheared.

9. The cadmium metal reduction and recovery method according to claim 1, characterized in that: Pretreatment of cadmium-containing materials to dry cadmium-containing materials includes: Put the cadmium-containing materials into the drying kiln, set the calcination temperature to 480-570℃, and keep it warm for 4.5-5.5 hours after the temperature in the kiln reaches 510℃.

10. A cadmium metal reduction system, characterized in that: The cadmium metal recovery method according to any one of claims 1 to 9 is used to recover cadmium metal, wherein the cadmium metal reduction system comprises: a reduction furnace, an alkali slag flake machine, a cadmium discharge chute assembly, an alkali slag discharge chute assembly, a heat preservation furnace, a crude cadmium material feed pipe, a distillation furnace, a refined cadmium discharge pipe, a vacuum assembly, a rod casting machine, a dust removal assembly and a drying kiln; The reduction furnace is connected to the alkali slag flaker through the alkali slag discharge chute assembly, and the reduction furnace is connected to the holding furnace through the cadmium discharge chute assembly, the holding furnace is connected to the distillation furnace through the crude cadmium material feed pipe, the distillation furnace is connected to the rod casting machine through the refined cadmium discharge pipe, and the vacuum assembly is connected to the distillation furnace, and the dust removal assembly is connected to the reduction furnace, the alkali slag flaker, the holding furnace and the rod casting machine.