Hard alloy with gradient symmetrical structure and preparation method and application thereof
Through the preparation method of cemented carbide with gradient symmetric structure, the gradient combination of Co powder and V(C,N) powder of different particle sizes is solved, and the problem of traditional cemented carbide is difficult to have high hardness and high toughness at the same time, realizing the material The external toughness and inner hardness are improved, suitable for the needs of modern manufacturing.
Patent Information
- Application Number
- CN202410988417.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
Traditional cemented carbides are difficult to have high hardness and high toughness at the same time, resulting in the inability to meet the cost and efficiency requirements of use in modern manufacturing, and are prone to performance attenuation or failure risks caused by material stratification.
The preparation method of cemented carbide with gradient symmetric structure is used to control the grain size and micromorphology after sintering through the gradient matching and distribution of Co powder and V(C,N) powder of different particle sizes to achieve the improvement of the mechanical properties of the material. , forming an effect of toughness on the outside and hard on the inside.
It achieves the overall performance improvement of the material, extends the service life, and improves the density and comprehensive performance of the material, and is suitable for scenarios with uniform stress in practical applications.
Smart Images

Figure CN118932207A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a hard alloy with a gradient symmetrical structure and a preparation method and application thereof, belonging to the field of hard alloy manufacturing. Background Art
[0002] Cemented carbide is a metal ceramic tool material prepared by powder metallurgy method with refractory metal compounds (WC, TiC, TaC, NbC, etc.) as hard phase and transition metals (Fe, Co, Ni) as bonding phase. It has the advantages of high strength, high hardness, good wear resistance and corrosion resistance, and is widely used in drilling, mining, cutting tools, wear-resistant parts and other fields. With the development of modern science and technology, the end users of the market have higher and higher requirements on the cost and efficiency of cemented carbide. It is difficult for traditional cemented carbide to have high hardness and high toughness at the same time, and it cannot meet the development needs of future manufacturing industry.
[0003] In the prior art, a gradient is usually formed by the mass ratio of WC powder to Co powder, that is, the surface layer has a high WC powder content and the bottom layer has a high Co powder content, so as to adjust the hardness and toughness of the cemented carbide. However, this easily leads to material stratification and easy detachment at the junction, and there is a risk of performance degradation or failure due to composition differences. Summary of the invention
[0004] In view of the shortcomings of the prior art, the first object of the present invention is to provide a method for preparing a cemented carbide with a gradient symmetrical structure. The preparation method of the present invention is simple and controllable and suitable for industrial production.
[0005] The second object of the present invention is to provide a hard alloy with a gradient symmetrical structure prepared by the above preparation method. The hard alloy with a gradient symmetrical structure provided by the present invention is tough on the outside and hard on the inside, and in actual application, the forces on many products are uniform and symmetrical, and the symmetrical structure of the present invention can be better applied.
[0006] The third object of the present invention is to provide the application of the cemented carbide with a gradient symmetrical structure prepared by the above preparation method.
[0007] In order to achieve the above object, the present invention adopts the following technical solution:
[0008] The invention discloses a method for preparing a hard alloy with a gradient structure, comprising: preparing two portions of mixed powder A, two portions of mixed powder B, and one portion of mixed powder C, spreading the powder in a manner that the mixed powder C is in the middle, the two portions of mixed powder B are respectively located on both sides of the mixed powder C, and the two portions of mixed powder A are respectively located above or below the two portions of mixed powder B to form a vertically symmetrical gradient powder, pressing and molding to obtain a compact, and sintering the compact to obtain a hard alloy;
[0009] The mixed powder A, mixed powder B and mixed powder C are all composed of WC powder, Co powder No. 1, Co powder No. 2, Co powder No. 3 and V (C, N) powder;
[0010] Among them, the particle size of Co powder No. 1 is 50-400nm, the particle size of Co powder No. 2 is 500-800nm, and the particle size of Co powder No. 3 is 9000-1500nm.
[0011] In the mixed powder A, the volume ratio of Co powder No. 1: Co powder No. 2: Co powder No. 3 is 40-60: 20-30: 10-30;
[0012] In the mixed powder B, the volume ratio of Co powder No. 1: Co powder No. 2: Co powder No. 3 is 20-30: 50-60: 20-30;
[0013] In the mixed powder C, the volume ratio is Co powder No. 1: Co powder No. 2: Co powder No. 3 = 10-30: 25-40: 40-60.
[0014] The preparation method of the present invention provides a hard alloy with a gradient structure, which has a gradient symmetrical structure. Co powders of different particles are used in each gradient layer to match each other to achieve maximum stacking complementarity between particles. Co powders of different sizes are used to control the grain size and micromorphology of the material after sintering and the degree of Co diffusion to achieve control of the mechanical properties of the material, achieve overall improvement of the material performance, achieve the effect of tough outside and hard inside, effectively improve the overall density of the material, extend the service life of the material, and make the material more suitable for practical use.
[0015] In the present invention, by controlling the use of different particles of Co powder in each gradient layer, the grain size and micromorphology of the sintered material and the degree of Co diffusion are controlled by Co powders of different sizes, and the Co content will undergo a gradient change, and Co will continuously migrate from the inside to the outside, thereby showing a trend of increasing Co from the inside to the outside, and the WC grains will become denser and finer, and there will be no abnormal growth of grains, and there will be fewer sources of fracture, so as to achieve a state of balanced force in the material structure in practical applications, and extend the service life. There is a cobalt-rich layer on the surface of the material, which has high toughness and can absorb the energy of crack growth, thereby effectively preventing further crack expansion. At the same time, due to the presence of the cobalt-rich layer on the surface, the heat dissipation capacity is greatly improved, and thermal stress can be effectively eliminated, which can improve the comprehensive performance and service life of cemented carbide.
[0016] However, Co powder also needs to be effectively controlled, and the maximum size cannot exceed 1.5μm. Otherwise, due to the obviously uneven distribution of Co phase in the compact, on the one hand, the critical degree of WC is increased, the merger between WC is aggravated, and the WC grains are enlarged. On the other hand, the degree of dissolution, precipitation and recrystallization of local WC is increased, resulting in abnormal growth of individual grains, more grains larger than 6μm, and a higher probability of abnormal grain growth. Of course, Co powder cannot be too small. If it is too small, the Co powder is too fine, the surface energy of the Co phase is larger, and the liquid phase appears earlier during the sintering process. Under the same sintering process, the liquid phase amount and liquid phase sintering time are increased, which aggravates the dissolution, precipitation and recrystallization of WC, and also promotes the abnormal growth of WC grains.
[0017] In a preferred embodiment, in the mixed powder A, the mass fraction of V(C,N) powder is 0.4-0.5wt.%, preferably 0.45-0.5%; in the mixed powder B, the mass fraction of V(C,N) powder is 0.25-0.35wt.%, preferably 0.3-0.35%; in the mixed powder C, the mass fraction of V(C,N) powder is 0.2-0.3wt.%, preferably 0.2-0.25%.
[0018] In the present invention, a small amount of V(C,N) powder is added to each powder as a grain inhibitor to control the grain size and micromorphology, and the grain inhibitor is also distributed in a gradient. The V(C,N) powder is added in the largest amount in the mixed powder A laid on the top and bottom layers (both forming the surface layer of the compact), and the V(C,N) powder is added in the smallest amount in the mixed powder C laid in the middle. The inventors found that the grain inhibitor gradient can control the Co diffusion of the material during the sintering process, and the grain inhibitor gradient can also promote Co diffusion, further increase the thickness of the material gradient layer, promote diffusion, and make the material undergoing diffusion reaction more , which is reflected in the material as the diffusion layer becomes thicker, making the gradient change of the material more uniform and thorough, effectively improving the overall mechanical properties of the material. During the sintering process of gradient cemented carbide, V (C, N) is constantly decomposed, N atoms migrate to the surface, and V migrates to the inside under the thermal coupling mechanism. This migration mechanism causes vacancies on the alloy surface due to the migration of V atoms, which are then filled by atoms of the bonding phase (Co), thereby forming a layer of bonding phase-rich area on the alloy surface. On the other hand, the V atoms that migrate to the interior of the alloy recombine with the internal carbon, nitrogen and other atoms to generate new hard phase nitrides or carbonitrides. This process not only refines the grain structure inside the alloy, but also enhances the hardness and wear resistance of the alloy through the redistribution of V atoms and the formation of compounds.
[0019] On the one hand, the present invention accelerates the above process and further promotes diffusion by setting the gradient difference of V(C, N); and by creating the V(C, N) gradient, the diffusion phenomenon can be promoted, the V(C, N) cubic phase is accelerated to dissolve, and the cubic phase is reduced. On the other hand, by controlling the mass fraction of the V(C, N) powder in the outermost layer, i.e., the mixed powder A, within the scope of the present invention, excessive loss of Co can be avoided; at the same time, since the evaporation rate is inversely proportional to the powder particle size, the particle size gradient of Co in the present invention can also effectively alleviate the loss problem of Co.
[0020] If the composition gradient is controlled alone and the mass fraction of V(C,N) powder in the mixed powder A is unreasonable, the thermal stability of V(C,N) is not high and the reaction is too rapid, which will lead to premature enrichment of Co on the surface, resulting in easy evaporation and loss, forming a cobalt-poor surface layer. Cobalt-poor will lead to reduced surface toughness, and Co as a bonding phase will cause the surface to fall off easily, resulting in more severe tool wear, reduced cutting performance, and rapid tool failure.
[0021] In addition, the inventors found that in the present invention, the combination of Co particle size is also beneficial to the diffusion of V(C,N) and can promote its dissolution, thereby playing a role in improving the solubility of the grain inhibitor. Because in the present invention, there are more large particles of internal Co, similar to "a large proportion of coarse powder", which can provide more channels for the migration of V. Because the diffusion driving force is smaller as it goes deeper into the interior, it is very important to provide diffusion channels inside. At the same time, due to the migration of V, it can limit the tendency of abnormal grain growth. Therefore, in the present invention, the combination of Co particle size and the addition of V(C,N) grain inhibitor can further refine the grains and enhance the performance of the material.
[0022] In the present invention, the vanadium carbonitride powder is used, which is a carbon-containing product in the vanadium nitride product, wherein the mass fractions of the components are: V is 79%, N is 12%, and C is 7%.
[0023] In a preferred embodiment, in the mixed powder A, mixed powder B and mixed powder C, the sum of the mass fractions of Co powder No. 1, Co powder No. 2 and Co powder No. 3 is 8-12%.
[0024] In the present invention, the total mass fractions of Co powder No. 1, Co powder No. 2 and Co powder No. 3 in the three mixed powders are the same. The inventors found that this can make the performance of the obtained cemented carbide optimal. If the sum of the layers of Co powder changes significantly, it is actually similar to "stitching" different materials together, and the following problems are prone to occur: Poor interlayer bonding: The splicing method is difficult to ensure the close bonding between different material layers, and it is easy to have poor interlayer bonding, which will affect the overall mechanical properties of the gradient material. Discontinuous microstructure: Since the splicing method is to directly combine different materials together, it is difficult to achieve a continuous transition of materials at the microstructure level, which will affect the performance uniformity of the gradient material. Difficult to adapt to complex structures: For gradient materials with complex structures or shapes, the direct splicing method may be difficult to achieve precise matching and combination, limiting its application in complex structures.
[0025] In addition, the Co content also needs to be controlled within the scope of the present invention to obtain the optimal performance. If there is too much Co, the following problems are likely to occur: 1. Reduced hardness: When the Co content exceeds a certain range (such as more than 20%), the Co phase may occupy too much space in the alloy, resulting in reduced direct contact between WC particles, thereby reducing the hardness of the alloy. 2. Reduced wear resistance: Too much Co phase may reduce the wear resistance of the alloy because the hardness of Co itself is lower than that of WC. During the wear process, too much Co phase may be more easily worn away. 3. Affecting toughness: Although the Co phase can improve the toughness of the alloy, too much Co phase may cause the alloy to be too soft, reducing its impact resistance and fracture resistance. When the Co content is too low, the following problems will also occur: 1. Reduced bonding strength: Co acts as a binder to bond WC particles together. If the Co content is too low, it may cause the bonding between WC particles to be loose, thereby reducing the overall strength and toughness of the alloy. 2. Affecting the coating quality: In the preparation process of WC-Co, the wettability of Co relative to WC particles is very important. If the Co content is too low, it may cause uneven distribution of WC particles and reduced quality. 3. Reduced corrosion resistance: The right amount of Co phase can reduce the intergranular gap of the alloy, increase the density and corrosion resistance of the alloy. However, too little Co content may cause the intergranular gap of the alloy to increase, thereby reducing its corrosion resistance.
[0026] Preferably, the thickness of layer C obtained by spreading the mixed powder C accounts for 45-50% of the thickness of the gradient powder; the thickness of layer B1 and layer B2 obtained by spreading the two mixed powders B account for 15-20% of the thickness of the gradient powder; the thickness of layer A1 and layer A2 obtained by spreading the two mixed powders A account for 5-15% of the thickness of the gradient powder.
[0027] In the present invention, by matching the particle size of Co powder and the gradient distribution of V (C, N) powder, layer A1 and layer A2 form the layers with the highest toughness, and layer C is the layer with the best hardness. By controlling the thickness of each layer within the scope of the present invention by spreading the powder, it can be ensured that layer C can cover the highest stress point and ensure that the material is in the best state.
[0028] In a preferred solution, the mixed powder A, mixed powder B and mixed powder C are all obtained by mixing raw material powders of each layer in proportion, performing wet ball milling, drying and sieving.
[0029] Further preferably, during the wet ball milling, anhydrous ethanol is used as the ball milling medium, the ball-to-material ratio is 8-12:1, the ball milling speed is 160-200 r / min, and the ball milling time is 36-50 h.
[0030] Further preferably, the drying is vacuum drying, and the vacuum drying time is 4-8 hours.
[0031] Preferably, the pressing pressure is 10-20t.
[0032] In a preferred embodiment, the sintering temperature is 1300-1500° C., the sintering time is 2-4 hours, and the sintering pressure is 4-6 MPa.
[0033] Further preferably, the sintering process is: first, in a vacuum degree of 10 -3 In a vacuum environment of 1000 pa, heat up to 550-650°C at a rate of 5-10°C / min, keep warm for 4-6 hours, then continue to heat up to 1150-1250°C, start to fill with protective atmosphere, make the pressure 4-6Mp, and heat up to 1300-1500°C, keep warm for 2-4 hours.
[0034] More preferably, the protective atmosphere is argon.
[0035] In the preferred sintering process, the present invention first performs vacuum pre-sintering at a low temperature to reduce the oxides on the powder surface, which is beneficial to the solid-phase reaction in the subsequent sintering process. At the same time, the pre-sintering process can reduce the contact stress between the powder particles, and the particles begin to diffuse on the surface, thereby improving the strength of the pressed block. Subsequently, the temperature is raised to the solid-phase sintering stage, and the solid-phase reaction and diffusion begin to intensify, the contact area between the powder particles increases, and a preliminary sintering neck is formed. At the same time, the bonding metal powder begins to recover and recrystallize, preparing for the subsequent liquid phase sintering. Finally, the temperature is raised to the liquid phase sintering stage, and atmosphere sintering is performed under pressure. At this time, the generation of the liquid phase promotes the rapid shrinkage and densification of the sintered body, the WC powder is dissolved, precipitated, and recrystallized, V (C, N) is continuously decomposed, N atoms migrate to the surface, and V migrates to the inside under the thermal coupling mechanism. Taking the inside as an example, generally speaking, the coarse powder has a smaller specific surface area, but the gaps between its particles are larger, which is beneficial to the transmission and diffusion of substances during the sintering process, but may reduce the density of the sintered body to a certain extent; in the present invention, the inside has more large particles of Co, similar to the "coarse powder ratio "Big", which can provide more channels for V migration (because the diffusion driving force is smaller the further inside, so it is very important to provide diffusion channels inside), and at the same time, due to the migration of V, it can limit the tendency of abnormal grain growth. The content of V outside is low, so at this time, we must pay great attention to the abnormal growth of grains (V can effectively inhibit growth). At this time, more fine powder is given to the outside of the material, and fine powder has a larger specific surface area, which can provide more sintering necks, thereby promoting the bonding between particles during the sintering process, improving the density of the sintered body and reducing the porosity. In the early stage of sintering, powder particles form sintering necks through surface diffusion and volume diffusion. Due to its large specific surface area, fine powder is more likely to form sintering necks and promote bonding between particles. With the increase of sintering temperature and time, the sintering necks gradually grow and connect adjacent particles to form a sintered body. The combination of coarse and fine powders can promote the progress of this process and optimize the structure of the sintered body. The fine powder promotes the surface diffusion of the material through its high specific surface area. The appropriate combination of coarse and fine powders can balance the transmission and diffusion process, so that the sintered body has a good pore structure and grain structure while maintaining a high density. The fine grains help to improve the toughness and strength of the material. At the same time, through the synergistic effect of the gradient coarse and fine combination of the present invention and the grain inhibitor, the final sintering obtains a gradient symmetrical structure with fine grains of the bonding phase increasing from the inside to the outside, so that the cemented carbide has the performance characteristics of being tough on the outside and hard on the inside.
[0036] The present invention also provides a hard alloy with a gradient structure prepared by the above preparation method.
[0037] The present invention also provides the application of the hard alloy with a gradient structure prepared by the above preparation method, and the hard alloy with a gradient structure is applied as a blank for a numerical control blade.
[0038] Beneficial Effects
[0039] The preparation method of the present invention provides a hard alloy with a gradient structure, which has a gradient symmetrical structure. Co powders of different particles are used in each gradient layer to match each other to achieve maximum stacking complementarity between particles. Co powders of different sizes are used to control the grain size and micromorphology of the material after sintering and the degree of Co diffusion to achieve control of the mechanical properties of the material, achieve overall improvement of the material performance, achieve the effect of tough outside and hard inside, effectively improve the overall density of the material, extend the service life of the material, and make the material more suitable for practical use. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 The surface scanning electron microscope photos of the cemented carbide samples obtained in the examples and comparative examples are shown in FIG. Figure 1 (a) is a surface scanning electron microscope photograph of the sample 1 prepared in Example 1 at a magnification (×2000), Figure 1 (b) is a surface scanning electron microscope photograph of the sample 1 prepared in Example 1 at a magnification (×10000). Figure 1 (c) is a surface scanning electron microscope photograph of the sample 1 prepared in comparative example 1 at a magnification (×2000), Figure 1 (d) is a surface scanning electron microscope photograph of sample 1 prepared in comparative example 1 at a magnification (×10000).
[0041] Figure 2 The figure is a comparison chart of the hardness HV experimental data of the cemented carbide samples obtained in Example 1 and Comparative Example 1.
[0042] Figure 3 The figure is a comparison chart of the HRA experimental data of the hardness of the cemented carbide samples obtained in Example 1 and three comparative examples.
[0043] Figure 4 Density experimental comparison chart of cemented carbide samples obtained in Example 1 and 3 comparative examples.
[0044] Figure 5 Comparison chart of the bending strength experiments of the cemented carbide samples obtained in Example 1 and Comparative Example 1.
[0045] Figure 6 A schematic diagram of the gradient structure of a cemented carbide sample provided by the present invention. DETAILED DESCRIPTION
[0046] Example 1
[0047] 1. According to Table 1, weigh different proportions of powders for ball milling, the ball-to-material ratio is 10:1, the wet grinding agent is anhydrous ethanol (40wt.%), the rotation speed is 180r / min, ball milling for 48h, vacuum drying for 6h, and sieving to obtain mixed powder.
[0048] 2. Spread the powder according to the proportion in Table 2, and press after obtaining a vertically symmetrical gradient powder structure with a pressing pressure of 15t.
[0049] 3. Perform vacuum pressure sintering with a heating rate of 5°C / min and a vacuum degree of 10 -3 pa, heat to 600℃ and keep it for 4h, then continue to heat to 1200℃, then start to inject 5Mpa argon, and heat to 1400℃ at 5℃ / min, keep it at this temperature and pressure for 2h, then cool it with the furnace to obtain sample 1.
[0050] Table 1 Composition of each layer of Example 1
[0051]
[0052] Comparative Example 1
[0053] 1. According to Table 1, weigh the powder and perform ball milling, the ball-to-material ratio is 10:1, the wet grinding agent is anhydrous ethanol (40wt.%), the rotation speed is 180r / min, ball milling for 48h, vacuum drying for 6h, and sieving to obtain mixed powder.
[0054] 2. Pressing is carried out with a pressing pressure of 15t.
[0055] 3. Perform vacuum pressure sintering with a heating rate of 5°C / min and a vacuum degree of 10 -3 pa, heat to 600℃ and keep it for 4h, then continue to heat to 1200℃, then start to inject 5Mpa argon, and heat to 1400℃ at 5℃ / min, keep it at this temperature and pressure for 2h, then cool it with the furnace to obtain sample 2.
[0056] Table 2 Composition of comparative example 1
[0057]
[0058] Experimental results of Example 1 and Comparative Example 1:
[0059] Metallographic photos: Figure 1 It can be seen that the grains of sample 1 are finer, more evenly distributed, with fewer pores, and no obvious defects such as cobalt pools.
[0060] Hardness test: Figure 2It can be seen that the HV hardness of sample 1 (average value is 2350) is higher than that of sample 2 (average value is 2050). This is because the hardness increases with the decrease of grain size. Sample 2 has more pores and larger grains, and there is abnormal grain growth. Therefore, the hardness of sample 1 is obviously better.
[0061] Density test: From Figure 4 It can be seen that the density of sample 1 (average value is 14.8) is higher than the density of sample 2 (average value is 14.4). This is because the preparation method of the present invention suppresses the formation of the cubic phase, while the traditional production method (sample 2) cannot prevent the formation of the cubic phase, and the solubility of V (C, N) is low, so there is a certain difference in density.
[0062] Bending strength test: Figure 5 It can be seen that the flexural strength of sample 1 (average value is 4500) is higher than that of sample 2 (average value is 4100). This is because within a certain range, as the WC grains become finer, there is a specific area where the flexural strength increases with the grain size. The sample prepared by this method has finer grains, more uniform distribution, fewer pores, and no obvious defects such as cobalt pools, so it has better flexural strength.
[0063] Comparative Example 2:
[0064] The other conditions are the same as those in Example 1. The content of V(C,N) powder in the mixed powder A is 0.2%, and Figure 3 It can be seen that the hardness of Comparative Example 2 is much lower than that of Example 1, which is mainly due to the formation of a cobalt-poor layer on the surface.
[0065] Comparative Example 3:
[0066] Other conditions are the same as those in Example 1, except that the thickness of layer C obtained by spreading the mixed powder C accounts for 10% of the thickness of the gradient powder; the thickness of layer B1 and layer B2 obtained by spreading the two mixed powders B accounts for 10% of the thickness of the gradient powder, and the thickness of layer A1 and layer A2 obtained by spreading the two mixed powders A accounts for 35% of the thickness of the gradient powder. Figure 3 , Figure 4 It can be seen that both the hardness and density are lower than those in Example 1. This is because the inner layer of the gradient cemented carbide formed by the above thickness is thinner and the outer layer is thicker, resulting in uneven residual stress distribution and significant performance differences, while the density is lower. This distribution will result in more cubic phases, reducing the overall density.
Claims
1. A method for preparing a hard alloy with a gradient structure, characterized in that: Prepare two portions of mixed powder A, two portions of mixed powder B, and one portion of mixed powder C, spread the powder in a manner that the mixed powder C is in the middle, the two portions of mixed powder B are located on both sides of the mixed powder C, and the two portions of mixed powder A are located above or below the two portions of mixed powder B to form a vertically symmetrical gradient powder, press and shape to obtain a compact, and sinter the compact to obtain a cemented carbide; The mixed powder A, mixed powder B and mixed powder C are all composed of WC powder, Co powder No. 1, Co powder No. 2, Co powder No. 3 and V (C, N) powder; Among them, the particle size of Co powder No. 1 is 50-400nm, the particle size of Co powder No. 2 is 500-800nm, and the particle size of Co powder No. 3 is 9000-1500nm. In the mixed powder A, the volume ratio of Co powder No. 1: Co powder No. 2: Co powder No. 3 is 40-60: 20-30: 10-30; In the mixed powder B, the volume ratio of Co powder No. 1: Co powder No. 2: Co powder No. 3 is 20-30: 50-60: 20-30; In the mixed powder C, the volume ratio is Co powder No. 1: Co powder No. 2: Co powder No. 3 = 10-30: 25-40: 40-60.
2. The method for preparing a cemented carbide with a gradient structure according to claim 1, characterized in that: In the mixed powder A, the mass fraction of V(C, N) powder is 0.4-0.5wt.%, in the mixed powder B, the mass fraction of V(C, N) powder is 0.25-0.35wt.%, and in the mixed powder C, the mass fraction of V(C, N) powder is 0.2-0.3wt.%.
3. The method for preparing a cemented carbide with a gradient structure according to claim 1, characterized in that: In the mixed powder A, mixed powder B and mixed powder C, the sum of the mass fractions of Co powder No. 1, Co powder No. 2 and Co powder No. 3 is 8-12%.
4. The method for preparing a cemented carbide with a gradient structure according to claim 1, characterized in that: The thickness of layer C obtained by spreading the mixed powder C accounts for 45-50% of the thickness of the gradient powder; the thickness of layers B1 and B2 obtained by spreading the two mixed powders B account for 15-20% of the thickness of the gradient powder; the thickness of layers A1 and A2 obtained by spreading the two mixed powders A account for 5-15% of the thickness of the gradient powder.
5. The method for preparing a cemented carbide with a gradient structure according to claim 1, characterized in that: The mixed powder A, mixed powder B and mixed powder C are obtained by mixing raw material powders of each layer in proportion, performing wet ball milling, drying and sieving; During the wet ball milling, anhydrous ethanol is used as the ball milling medium, the ball-to-material ratio is 8-12:1, the ball milling speed is 160-200 r / min, and the ball milling time is 36-50 h; The drying is vacuum drying, and the vacuum drying time is 4-8 hours.
6. The method for preparing a cemented carbide with a gradient structure according to claim 1, characterized in that: The pressing pressure is 10-20t.
7. The method for preparing a cemented carbide with a gradient structure according to claim 1, characterized in that: The sintering temperature is 1300-1500° C., the sintering time is 2-4 hours, and the sintering pressure is 4-6 MPa.
8. The method for preparing a cemented carbide with a gradient structure according to claim 7, characterized in that: The sintering process is as follows: first, the vacuum degree is 10 -3 In a vacuum environment of 1000 pa, heat up to 550-650°C at a rate of 5-10°C / min, keep warm for 4-6 hours, then continue to heat up to 1150-1250°C, start to fill with protective atmosphere, make the pressure 4-6Mp, and heat up to 1300-1500°C, keep warm for 2-4 hours.
9. A cemented carbide with a gradient structure prepared by the preparation method according to any one of claims 1 to 8.
10. Application of a hard alloy with a gradient structure prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The cemented carbide with the gradient structure is used as a CNC blade blank.