High-performance copper alloy strip for new energy vehicle-mounted connector and preparation method
By adding rare earth elements yttrium and lanthanum to the copper alloy strip and using multiple annealing, rolling and grinding processes, the problem of poor stress relaxation resistance of copper alloy strips is solved, and the preparation of high-performance copper alloy strips is realized , improves tensile strength and yield strength, while ensuring performance stability and material yield.
Patent Information
- Application Number
- CN202411425760.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-14
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing copper alloy strips have poor stress relaxation resistance, and the bright annealing and single-solution processes after rolling during the preparation process cannot ensure the stability of the strip performance.
Using specific proportional ingredients of Ti, Fe, Y, La and other elements, high-performance copper alloy belts are prepared through vacuum smelting, hot rolling, milling surface, cold rolling, bell furnace annealing, multiple solid solution and grinding processes. Materials, including multiple annealing, rolling and grinding processes to improve performance stability.
The tensile strength ≥920MPa and the yield strength ≥870MPa were achieved, which maintains high hardness and has good bending performance and elongation, significantly improves stress relaxation resistance, solves performance stability problems and improves material yield.
Smart Images

Figure CN118932212A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of copper alloy strip preparation, and in particular to a high-performance copper alloy strip for a new energy vehicle connector and a preparation method thereof. Background Art
[0002] High-performance copper alloy strips for new energy vehicle connectors are key materials for connectors in new energy vehicles. Connectors play a vital role in new energy vehicles because they are responsible for transmitting power, signals and other key data to ensure the normal operation of the vehicle. High-performance copper alloy strips can improve the electrical conductivity, thermal conductivity, corrosion resistance and oxidation resistance of connectors, thereby improving the performance and reliability of the entire vehicle.
[0003] A copper alloy strip and a preparation method thereof with the authorization publication number CN113005326B, wherein the mass percentage composition of the copper alloy strip is Fe: 7-11wt%, P: 0.006-0.012wt%, Sn: 0.5-1.5wt%, Ni: 4-6wt%, and the balance is copper and unavoidable impurities. By controlling the addition content of elements such as Fe, Sn, Ni, and P, the Fe-rich phase exists in the form of a skeleton in the copper matrix, which plays a role in improving strength and bending. The copper alloy strip has a tensile strength of 700-850 MPa, a conductivity of ≥25% IACS, an elongation of more than 10%, a 90° bending R / t of GW≤0.5, a BW≤1.5, and a hardness of 80% of the original hardness when kept at 500°C for 5 minutes. The copper alloy strip has poor stress relaxation resistance, and the preparation process is bright annealing after rolling. The single annealing and solution treatment process cannot guarantee the stable performance of the strip.
[0004] In order to solve the above problems, a high-performance copper alloy strip for a new energy vehicle connector and a preparation method thereof are proposed. Summary of the invention
[0005] The purpose of the present invention is to provide a high-performance copper alloy strip for new energy vehicle connectors and a preparation method, which solves the problem that the existing copper alloy strip in the background technology has poor stress relaxation resistance, and the preparation process is bright annealing after rolling, and the single annealing and solid solution process cannot ensure the stable performance of the strip.
[0006] To achieve the above object, the present invention provides the following technical solution: A high-performance copper alloy strip for a new energy vehicle connector, comprising the following components: Ti: 2.0%~3.5%; Fe: 0.15%~0.2%; Y: 0%~0.08%; La: 0%~0.08%; The remainder is Cu; Among them, Cu+Ti+Fe+Y+La≥99.5%.
[0007] Another technical solution proposed by the present invention is to provide a high-performance copper alloy strip for a new energy vehicle connector and a preparation method thereof, comprising the following steps: S1: batching: batching high-performance copper alloy strip with Cu, Ti, Fe, Y and La according to proportions; S2: Melting and casting: Vacuum melting at a temperature of 1200-1300°C. After vacuum degassing and melting, the billet is made into a casting billet by a semi-continuous casting process; S3: hot rolling: hot rolling the ingot, the initial rolling temperature of the hot rolling is 800-950°C, the total processing rate of the hot rolling is 85-95%, and the plate alloy is obtained; S4: Milling: The hot-rolled plate is milled twice with a milling amount of 2.5mm on one side and 0.3mm on one side. The two milling processes can better remove the oxidized components on the alloy surface.
[0008] S5: Cold rolling: The milled alloy is subjected to rough rolling to form a blank. The rough rolling is divided into 11 passes, and the total processing rate is 70-80%; S6: Bell furnace annealing: annealing treatment is carried out at 400-700℃ for 4-6h to eliminate subsequent work hardening, ensure smooth rolling and eliminate the impact of cracking; S7: Intermediate rolling: The annealed alloy is subjected to intermediate rolling, which is divided into 7 passes with a total processing rate of 65-75%; S8: Solution treatment: subjecting the alloy rolled to 0.9 mm to solution treatment, wherein the temperature of the solution treatment is preferably 800-900° C., and the speed of the solution treatment is preferably 10-20 m / min; S9: Pickling and grinding: The alloy strip after solid solution is pickled and ground, and a non-woven titanium roller polishing brush made of silicon carbide is used for grinding; S10: Pre-finish rolling: The cleaned and ground strip is pre-finish rolled to a bottom thickness of 0.103mm. There are 9 pre-finish rolling passes in total, with a total processing rate of 80-90%; S11: Solution treatment: subjecting the alloy rolled to 0.103 mm to solution treatment, wherein the temperature of the solution treatment is preferably 800-900° C. and the speed of the solution treatment is preferably 40-55 m / min; S12: cleaning and grinding: the alloy strip after solid solution is pickled and ground, and a non-woven titanium roller polishing brush made of silicon carbide is used for grinding; S13: Finish rolling: The ground alloy is subjected to finish rolling treatment in a rolling mill with a working roll roughness of less than 0.1 μm, and rolled to a finished product of 0.08 mm; S14: Aging treatment: In order to ensure the performance of the finished product, bell furnace aging is required. The aging temperature range is 400-600℃, the aging insulation is 4-6h, and the aging atmosphere is pure nitrogen atmosphere; S15: Finished product pickling: After the finished product is aged, in order to ensure the surface of the product, the finished product needs to be pickled, and a non-woven titanium roller polishing brush made of silicon carbide is used for grinding; S16: Straightening: The finished product after pickling is straightened. The tension range of straightening uncoiling is between 15-20KN and the tension range of straightening uncoiling is between 50-65KN. S17: Edge trimming and striping: Edge trimming of finished products, and edge trimming and striping of finished products after straightening.
[0009] Furthermore, the initial hot rolling temperature in S3 is 800-950° C., and the passes are distributed as follows: 130 mm→110 mm→91 mm→75 mm→61 mm→49 mm→39 mm→31 mm→25 mm→16 mm→12 mm→10.5 mm.
[0010] Furthermore, the 11 passes of rough rolling in S5 are as follows: 9.3mm→8.5mm→7.4mm→6.6mm→5.9mm→5.3mm→4.7mm→4.1mm→3.6mm→3.1mm→2.7mm→2.5mm, the rolling speed is 15-40m / min, and the tension range is 40-50KN.
[0011] Furthermore, the 7 passes of the intermediate rolling in S7 are distributed as follows: 2.5mm→2.15mm→1.85mm→1.6mm→1.37mm→1.18mm→1.03mm→0.9mm, the rolling speed is 70-100m / min, and the tension range is 20-30KN.
[0012] Furthermore, the silicon carbide grinding brush pressure current in the S9 is preferably 6-8A, the running belt speed is controlled between 10-14m / min, the drying box temperature is 80-90℃; the degreasing box temperature is 50-70℃; the passivation box temperature is 60-80℃; pay attention to removing the oxide layer on the surface of the alloy during grinding, and repeat grinding 2-3 times.
[0013] Furthermore, the 9 pre-finishing passes of S10 are distributed as follows: 0.9mm→0.71mm→0.57mm→0.45mm→0.34mm→0.27mm→0.21mm→0.165mm→0.131mm→0.103mm, the rolling speed is 150-200m / min, the tension range is 5-15KN, and if edge cracking is found during the rolling process, edge trimming is required, and rolling can be continued after edge trimming.
[0014] Furthermore, the silicon carbide grinding brush pressure current in the S12 is preferably 8-10A, the running belt speed is controlled between 9-13m / min, the drying box temperature is 80-90℃; the degreasing box temperature is 50-70℃; the passivation box temperature is 60-80℃, the surface oxide layer of the alloy needs to be removed, and the grinding is repeated 2-3 times.
[0015] Furthermore, the two passes of the finishing rolling in S13 are distributed as follows: 0.103 mm→0.085 mm→0.08 mm, the rolling speed is 200-240 m / min, and the tension range is 5-10 KN.
[0016] Furthermore, the grinding brush mesh number in S15 is 3000 mesh, the grinding brush pressure current is preferably 9-10A, the running belt speed is controlled between 60-70m / min, the drying box temperature is 80-90℃; the degreasing box temperature is 80-90℃; the passivation box temperature is 80-90℃.
[0017] Compared with the prior art, the present invention has the following beneficial effects: 1. The present invention provides a high-performance copper alloy strip for new energy vehicle connectors and a preparation method thereof. By adding rare earth elements yttrium and lanthanum and controlling the volume fraction of a specific texture, the alloy has a tensile strength of ≥920 MPa and a yield strength of ≥870 MPa. While maintaining high hardness, it also has good bending performance, elongation and stress relaxation resistance, thus solving the problem of poor stress relaxation resistance of existing copper alloy strips.
[0018] 2. The present invention provides a high-performance copper alloy strip for new energy vehicle connectors and a preparation method thereof, which is prepared through the following processes: batching → melting and casting → hot rolling → milling → cold rolling → bell furnace annealing → intermediate rolling → solution treatment → pickling and grinding → pre-finishing rolling → solution treatment → cleaning and grinding → finishing rolling → aging treatment → finished product pickling → bending and straightening → trimming and stripping, and adopts multiple annealing, rolling, solution treatment and grinding processes, which ensures the performance of the strip and effectively solves the difficulties of the cold rolling process of titanium-copper alloy, greatly improves the yield rate, lays a solid foundation for the mass production of subsequent products, and solves the problem that the existing copper alloy strip preparation process is to perform bright annealing after rolling, and the single annealing and solution treatment process cannot ensure the stable performance of the strip. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is a schematic diagram of the preparation process of the present invention; Figure 2 This is a data table of repeated direct aging tests on the thickness of the rolled product of the present invention. DETAILED DESCRIPTION
[0020] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0021] In order to solve the technical problems that the existing copper alloy strip has poor stress relaxation resistance and the preparation process is bright annealing after rolling, and the single annealing and solution process cannot ensure the stable performance of the strip, such as Figure 1-Figure 2 As shown, the following preferred technical solutions are provided: A high-performance copper alloy strip for a new energy vehicle connector, comprising the following components by mass percentage: Ti: 2.0%~3.5%; Fe: 0.15%~0.2%; Y: 0%~0.08%; La: 0%~0.08%; The remainder is Cu; Among them, Cu+Ti+Fe+Y+La≥99.5%. This strip achieves a tensile strength ≥920Mpa and a yield strength ≥870MPa by adding rare earth elements yttrium and lanthanum and controlling the specific texture volume fraction. It has good bending performance, elongation and stress relaxation resistance while maintaining high hardness, and has excellent comprehensive properties.
[0022] In order to further better explain the above embodiment, the present invention also provides an implementation scheme, a method for preparing a high-performance copper alloy strip for a new energy vehicle connector, comprising the following steps: Step 1: batching: Cu, Ti, Fe, Y and La are batched into high-performance copper alloy strip according to the proportion; Step 2: Melting and casting: Vacuum melting at a temperature of 1200-1300°C, the blank is subjected to vacuum degassing and melting, and then a semi-continuous casting process is used to obtain a cast blank; Step 3: hot rolling: hot rolling the ingot, the initial rolling temperature of the hot rolling is 800-950°C, the total processing rate of the hot rolling is 85-95%, and the plate alloy is obtained; Step 4: Milling: Mill the hot-rolled plate twice with a milling amount of 2.5mm on one side and 0.3mm on one side. The two millings can better remove the oxidized components on the alloy surface.
[0023] Step 5: Cold rolling: The milled alloy is subjected to rough rolling to form a blank. The rough rolling is divided into 11 passes, and the total processing rate is 70-80%; Step 6: Bell furnace annealing: annealing treatment is carried out at 400-700℃ for 4-6 hours to eliminate subsequent work hardening, ensure smooth rolling and eliminate the impact of cracking; Step 7: Intermediate rolling: The annealed alloy is subjected to intermediate rolling, which is divided into 7 passes with a total processing rate of 65-75%; Step 8: Solution treatment: The alloy rolled to 0.9 mm is subjected to solution treatment. The temperature of the solution treatment is preferably 800-900°C, and the speed of the solution treatment is preferably 10-20 m / min. Step 9: Pickling and grinding: Pickle and grind the alloy strip after solid solution, and use a non-woven titanium roller polishing brush made of silicon carbide for grinding; Step 10: Pre-finish rolling: The cleaned and ground strip is pre-finish rolled to a bottom thickness of 0.103mm. There are 9 pre-finish rolling passes in total, with a total processing rate of 80-90%; Step 11: Solution treatment: The alloy rolled to 0.103 mm is subjected to solution treatment. The temperature of the solution treatment is preferably 800-900°C; the speed of the solution treatment is preferably 40-55 m / min; Step 12: Cleaning and grinding: The alloy strip after solid solution is pickled and ground, and a non-woven titanium roller polishing brush made of silicon carbide is used for grinding; Step 13: Finish rolling: The ground alloy is subjected to finish rolling treatment in a rolling mill with a working roll roughness of less than 0.1 μm, and rolled to a finished product of 0.08 mm; Step 14: Aging treatment: In order to ensure the performance of the finished product, bell furnace aging is required, the aging temperature range is 400-600℃, the aging insulation is 4-6h, and the aging atmosphere is pure nitrogen atmosphere; Step 15: Pickling of finished products: In order to ensure the surface of the product after aging, the finished product needs to be pickled, and a non-woven titanium roller polishing brush made of silicon carbide is used for grinding; Step 16: Straightening: The finished product after pickling is straightened. The tension range of straightening uncoiling is between 15-20KN, and the tension range of straightening uncoiling is between 50-65KN. Step 17: Edge trimming and striping: Edge trimming of finished product, and edge trimming and striping of finished product after straightening.
[0024] The initial hot rolling temperature in step three is 800-950°C, and the passes are distributed as follows: 130mm→110mm→91mm→75mm→61mm→49mm→39mm→31mm→25mm→16mm→12mm→10.5mm.
[0025] The 11 passes of rough rolling in step 5 are as follows: 9.3mm→8.5mm→7.4mm→6.6mm→5.9mm→5.3mm→4.7mm→4.1mm→3.6mm→3.1mm→2.7mm→2.5mm, the rolling speed is 15-40m / min, and the tension range is 40-50KN.
[0026] The 7 passes of medium rolling in step seven are distributed as follows: 2.5mm→2.15mm→1.85mm→1.6mm→1.37mm→1.18mm→1.03mm→0.9mm, the rolling speed is 70-100m / min, and the tension range is 20-30KN.
[0027] The silicon carbide grinding brush pressure current in step nine is preferably 6-8A, the running belt speed is controlled between 10-14m / min, the drying box temperature is 80-90℃; the degreasing box temperature is 50-70℃; the passivation box temperature is 60-80℃; pay attention to remove the surface oxide layer of the alloy during grinding, and repeat grinding 2-3 times.
[0028] The 9 pre-finishing passes of step ten are distributed as follows: 0.9mm→0.71mm→0.57mm→0.45mm→0.34mm→0.27mm→0.21mm→0.165mm→0.131mm→0.103mm, the rolling speed is 150-200m / min, the tension range is 5-15KN, if cracking is found during the rolling process, trimming is required, and rolling can be continued after trimming.
[0029] The silicon carbide grinding brush pressure current in step twelve is preferably 8-10A, the running belt speed is controlled between 9-13m / min, the drying box temperature is 80-90℃; the degreasing box temperature is 50-70℃; the passivation box temperature is 60-80℃, the surface oxide layer of the alloy needs to be removed, and the grinding is repeated 2-3 times.
[0030] In step thirteen, the two passes of finishing rolling are distributed as follows: 0.103mm→0.085mm→0.08mm, the rolling speed is 200-240m / min, and the tension range is 5-10KN.
[0031] The grinding brush mesh number in step 15 is 3000 mesh, the grinding brush pressure current is preferably 9-10A, the running belt speed is controlled between 60-70m / min, the drying box temperature is 80-90℃; the degreasing box temperature is 80-90℃; the passivation box temperature is 80-90℃.
[0032] This process not only ensures the performance of the strip through multiple annealing and solution processes, but also effectively solves the difficulties of the cold rolling process of titanium-copper alloy, greatly improves the yield rate, and lays a solid foundation for the mass production of subsequent products. The strip prepared by this preparation method finally achieves tensile strength ≥920Mpa; yield strength ≥870MP; conductivity ≥15%; elongation ≥10%; elastic modulus ≥130Mpa; hardness >285HV.
[0033] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0034] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A high-performance copper alloy strip for new energy vehicle connectors, characterized in that: The high-performance copper alloy strip for new energy vehicle connectors includes the following components by mass percentage: Ti: 2.0%~3.5%; Fe: 0.15%~0.2%; Y:0%~0.08%; La: 0%~0.08%; The remainder is Cu; Among them, Cu+Ti+Fe+Y+La≥99.5%.
2. A method for preparing a high-performance copper alloy strip for a new energy vehicle connector according to claim 1, characterized in that: Preparation method The following steps are involved: S1: batching: batching high-performance copper alloy strip with Cu, Ti, Fe, Y and La according to proportions; S2: Melting and casting: Vacuum melting at a temperature of 1200-1300°C. After vacuum degassing and melting, the billet is made into a casting billet by a semi-continuous casting process; S3: hot rolling: hot rolling the ingot, the initial rolling temperature of the hot rolling is 800-950°C, the total processing rate of the hot rolling is 85-95%, and the plate alloy is obtained; S4: Milling: The hot-rolled plate is milled twice with a milling amount of 2.5 mm on one side and 0.3 mm on one side; S5: Cold rolling: The milled alloy is subjected to rough rolling to form a blank. The rough rolling is divided into 11 passes, and the total processing rate is 70-80%; S6: bell furnace annealing: annealing treatment is performed at 400-700°C for 4-6 hours; S7: Intermediate rolling: The annealed alloy is subjected to intermediate rolling, which is divided into 7 passes with a total processing rate of 65-75%; S8: Solution treatment: subjecting the alloy rolled to 0.9 mm to solution treatment, wherein the temperature of the solution treatment is preferably 800-900° C., and the speed of the solution treatment is preferably 10-20 m / min; S9: Pickling and grinding: The alloy strip after solid solution is pickled and ground, and a non-woven titanium roller polishing brush made of silicon carbide is used for grinding; S10: Pre-finish rolling: The cleaned and ground strip is pre-finish rolled to a bottom thickness of 0.103 mm. The pre-finish rolling is performed for a total of 9 passes, with a total processing rate of 80-90%; S11: Solution treatment: subjecting the alloy rolled to 0.103 mm to solution treatment, wherein the temperature of the solution treatment is preferably 800-900° C. and the speed of the solution treatment is preferably 40-55 m / min; S12: cleaning and grinding: the alloy strip after solid solution is pickled and ground, and a non-woven titanium roller polishing brush made of silicon carbide is used for grinding; S13: Finish rolling: The ground alloy is finished by rolling in a rolling mill with a working roll roughness of less than 0.1 μm to a finished product of 0.08 mm. S14: Aging treatment: In order to ensure the performance of the finished product, bell furnace aging is required. The aging temperature range is 400-600℃, the aging insulation is 4-6h, and the aging atmosphere is pure nitrogen atmosphere; S15: Finished product pickling: In order to ensure the surface of the product after aging, the finished product needs to be pickled, and a non-woven titanium roller polishing brush made of silicon carbide is used for grinding; S16: Straightening: The finished product after pickling is straightened. The tension range of straightening uncoiling is between 15-20KN, and the tension range of straightening uncoiling is between 50-65KN. S17: Edge trimming and striping: Edge trimming of finished products, and edge trimming and striping of finished products after straightening.
3. A method for preparing a high-performance copper alloy strip for a new energy vehicle connector as claimed in claim 2, characterized in that: The initial hot rolling temperature in S3 is 800-950° C., and the passes are distributed as follows: 130 mm→110 mm→91 mm→75 mm→61 mm→49 mm→39 mm→31 mm→25 mm→16 mm→12 mm→10.5 mm.
4. A method for preparing a high-performance copper alloy strip for a new energy vehicle connector as claimed in claim 3, characterized in that: The 11 passes of rough rolling in S5 are as follows: 9.3mm→8.5mm→7.4mm→6.6mm→5.9mm→5.3mm→4.7mm→4.1mm→3.6mm→3.1mm→2.7mm→2.5mm, the rolling speed is 15-40m / min, and the tension range is 40-50KN.
5. A method for preparing a high-performance copper alloy strip for a new energy vehicle connector as claimed in claim 4, characterized in that: The 7 passes of the S7 rolling are distributed as follows: 2.5mm→2.15mm→1.85mm→1.6mm→1.37mm→1.18mm→1.03mm→0.9mm, the rolling speed is 70-100m / min, and the tension range is 20-30KN.
6. A method for preparing a high-performance copper alloy strip for a new energy vehicle connector as claimed in claim 5, characterized in that: The silicon carbide grinding brush pressure current in the S9 is preferably 6-8A, the running belt speed is controlled between 10-14m / min, the drying box temperature is 80-90℃; the degreasing box temperature is 50-70℃; the passivation box temperature is 60-80℃; pay attention to removing the oxide layer on the surface of the alloy during grinding, and repeat grinding 2-3 times.
7. A method for preparing a high-performance copper alloy strip for a new energy vehicle connector as claimed in claim 6, characterized in that: The 9 pre-finishing passes of S10 are distributed as follows: 0.9mm→0.71mm→0.57mm→0.45mm→0.34mm→0.27mm→0.21mm→0.165mm→0.131mm→0.103mm. The rolling speed is 150-200m / min, and the tension range is 5-15KN. If edge cracking is found during the rolling process, edge trimming is required, and rolling can be continued after edge trimming.
8. A method for preparing a high-performance copper alloy strip for a new energy vehicle connector as claimed in claim 7, characterized in that: The silicon carbide grinding brush pressure current in the S12 is preferably 8-10A, the running belt speed is controlled between 9-13m / min, the drying box temperature is 80-90℃; the degreasing box temperature is 50-70℃; the passivation box temperature is 60-80℃, the surface oxide layer of the alloy needs to be removed, and the grinding is repeated 2-3 times.
9. A method for preparing a high-performance copper alloy strip for a new energy vehicle connector as claimed in claim 8, characterized in that: The two passes of the finishing rolling in S13 are distributed as follows: 0.103 mm→0.085 mm→0.08 mm, the rolling speed is 200-240 m / min, and the tension range is 5-10 KN.
10. A method for preparing a high-performance copper alloy strip for a new energy vehicle connector according to claim 9, characterized in that: The mesh number of the grinding brush in S15 is 3000 meshes, the grinding brush pressure current is preferably 9-10A, the running belt speed is controlled between 60-70m / min, the drying box temperature is 80-90℃; the degreasing box temperature is 80-90℃; the passivation box temperature is 80-90℃.
Citation Information
Patent Citations
High-strength and high-elasticity copper-titanium alloy and manufacturing method thereof
CN113278844A
Copper alloy sheet material and method for producing the same
JP2014015679A
Cited By
Titanium-copper alloy preform capable of preventing interlayer scratch and rolling process
CN119144885A