Target material for preparing amorphous coated nanocrystalline alloy film and preparation method and application thereof

Through the high-entropy alloy targets and magnetron sputtering technology with specific ratios, the problem of difficult preparation of amorphous coated nanocrystalline alloy films is solved, and amorphous coated nanocrystalline alloys with high strength and excellent creep deformation resistance is achieved. Thin films significantly improve the mechanical properties of the material.

CN118932237APending Publication Date: 2024-11-12HENAN ACADEMY OF SCIENCES +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411031943.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art is difficult to directly obtain a biphasic structure alloy film with amorphous coated nanocrystals through magnetron sputtering technology, and the composition design of high-entropy alloy targets is difficult to regulate, resulting in a little amorphous phase distributed in the nanocrystals, making it difficult to prepare and have excellent results. Amorphous coated nanocrystalline alloy film with mechanical properties.

Method used

The targets are prepared by mechanical alloying and sintering processes using specific ratios of Cr, Mn, Fe, Co, and Ni high-entropy alloy targets, and the amorphous coated nanometers are deposited on a single crystal silicon substrate using magnetron sputtering technology. Crystal alloy film, adjust the atomic percentage and sputtering parameters of the target to form an amorphously coated nanocrystal biphasic structure with a nanocrystal grain size less than 10 nm.

Benefits of technology

Amorphous coated nanocrystalline alloy film with a strength of up to 8.95Gpa was successfully prepared, which significantly improved the hardness and creep deformation resistance of the material, and was simple in process and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004970149350000011
    Figure HDA0004970149350000011
  • Figure HDA0004970149350000012
    Figure HDA0004970149350000012
  • Figure HDA0004970149350000021
    Figure HDA0004970149350000021
Patent Text Reader

Abstract

The invention provides a target material for preparing an amorphous coated nanocrystalline alloy film, which comprises the following components in percentage by atom: 12-25% of Cr, 16-30% of Mn, 10-23% of Fe, 9-22% of Co and 10-26% of Ni, and the atomic percentages of Cr, Mn, Fe, Co and Ni are not equal. The invention further provides a preparation method of the target material. The invention further provides a preparation method of the amorphous coated nanocrystalline alloy film. The target material provided by the invention is high in purity and compact in structure, a thin film sputtered by using the target material has a biphase structure of amorphous coated nanocrystalline, the crystal grain size of a crystal phase of the thin film is less than 10nm, and the thickness of an amorphous layer is 1-3nm. According to the method, a foundation is laid for preparation of the nanocrystalline alloy film with excellent performance such as high stability and high strength, and the application range of the nanocrystalline alloy film is widened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of alloy target materials, and in particular to a target material for preparing an amorphous-coated nanocrystalline alloy film, a preparation method thereof and an application thereof. Background Art

[0002] Nanocrystalline materials (grain size d < 100nm) are mainly characterized by small grains in structure. The presence of a large number of grain boundaries makes nanocrystalline materials have high strength. However, due to the lack of long-range ordered crystal structure at the grain boundaries, it is very easy to cause deformation dominated by grain boundary softening mechanisms such as grain rotation, grain boundary sliding and grain boundary diffusion, resulting in a decrease in the mechanical properties of nanocrystalline materials. After introducing amorphous phases into the grain boundaries of nanocrystalline alloys, the deformation mechanism of the material changes from grain boundary activation mode to shear band activation mode, which is expected to significantly improve the reduction in material hardness and creep deformation resistance caused by the grain boundary softening mechanism.

[0003] However, it is difficult to prepare amorphous-coated nanocrystalline dual-phase structure films using a single traditional alloy material. As a new type of "chemically disordered" multi-component solid solution alloy (high entropy alloy) discovered on the basis of exploring amorphous alloys, its unique high lattice distortion, high elastic mismatch and slow diffusion effect, combined with the advantages of fast solidification cooling rate and high nucleation rate during magnetron sputtering coating, and easy formation of fine nanocrystals or amorphous structures, provide the possibility for the preparation of amorphous-coated nanocrystalline dual-phase materials. However, even if a high entropy alloy target is selected, it is difficult to directly obtain the dual-phase structure of amorphous-coated nanocrystalline through magnetron sputtering technology. It is easy to obtain nanocrystals by adjusting the magnetron sputtering parameters, or a small amount of amorphous phase is distributed in the nanocrystals. Therefore, the design of the high entropy alloy target composition determines whether an alloy film of amorphous-coated nanocrystalline can be prepared. Summary of the invention

[0004] The technical problem solved by the present invention is to provide a target material for preparing alloy films. The target material provided in the present application can be used to prepare alloy films with amorphous-coated nanocrystalline structures, and the alloy films have excellent mechanical properties.

[0005] In view of this, the present application provides a target material for preparing an amorphous-coated nanocrystalline alloy film, which includes, in atomic percentage, Cr: 12-25%, Mn: 16-30%, Fe: 10-23%, Co: 9-22%, Ni: 10-26%, and the atomic percentages of Cr, Mn, Fe, Co and Ni are not equal to each other.

[0006] Preferably, the content of Cr is 15-20%, and the content of Mn is 18-25%.

[0007] Preferably, the content of Fe is 12-22%, the content of Co is 11-20%, and the content of Ni is 12-24%.

[0008] The present application also provides a method for preparing the target material, comprising the following steps:

[0009] Cr, Mn, Fe, Co and Ni are mixed according to atomic percentage ratio and then mechanically alloyed to obtain alloy powder;

[0010] The alloy powder is sintered to obtain a target material.

[0011] Preferably, the preparation process of the alloy powder is specifically as follows:

[0012] Ultrasonic cleaning of the mixed powder prepared according to atomic percentage ratio for 20 to 40 minutes;

[0013] The cleaned powder is dried at a vacuum degree of 1×10 -4 Pa~1×10 -5 Pa, the drying temperature is 60-100°C, and the drying time is 3-8h;

[0014] The dried powder is ball-milled to obtain alloy powder.

[0015] Preferably, the step of obtaining the target material is specifically:

[0016] Pre-pressing the alloy powder to obtain an initial target material;

[0017] The initial target material is subjected to spark plasma sintering to obtain a target material.

[0018] Preferably, the pre-pressing pressure is 10 MPa to 20 MPa, and the pre-pressing time is 1 to 5 hours.

[0019] Preferably, the spark plasma sintering is carried out at 8×10 -4 Pa~5×10 -5 The spark plasma sintering is carried out under a vacuum degree of Pa, the pressure of the spark plasma sintering is 20-50MPa, the temperature of the spark plasma sintering is 600°C-1000°C, the heating rate before sintering and the cooling rate after sintering are 40°C / min-80°C / min respectively, and the sintering holding time is 10min-25min.

[0020] The present application also provides a method for preparing an amorphous-coated nanocrystalline alloy film, comprising:

[0021] The target material is magnetron sputtered on the substrate to obtain an amorphous-coated nanocrystalline alloy film;

[0022] The target material is the target material or the target material prepared by the preparation method.

[0023] Preferably, the substrate is single crystal silicon; the magnetron sputtering is intermittent magnetron sputtering, the power supply is a radio frequency power supply, the power is 80W to 120W, the single sputtering time is 10min to 20min, and the interval between two sputtering processes is 5min to 10min; the sputtering gas is argon with a purity of ≥99.999%, and the pressure in the sputtering chamber is 0.1Pa to 1Pa; the thickness of the alloy film is 500nm to 1μm, of which the thickness of the amorphous layer is 1nm to 3nm, and the grain size is less than 10nm.

[0024] The present application provides a target material for preparing an amorphous-coated nanocrystalline alloy film, which includes, in atomic percentage, Cr: 12-25%, Mn: 16-30%, Fe: 10-23%, Co: 9-22%, Ni: 10-26%, and the atomic percentages of Cr, Mn, Fe, Co and Ni are not equal to each other. The target material provided by the present application adjusts the ratio of Cr, Mn, Fe, Co and Ni so that the target material can obtain an alloy film with an amorphous-coated nanocrystalline dual-phase structure through magnetron sputtering, wherein the nanocrystalline grain size of the alloy film is less than 10nm, and the thickness of the amorphous layer is 1nm-3nm; when the alloy film is 1μm, the strength is as high as 8.95Gpa, which is significantly higher than other high entropy alloy films, and has excellent creep deformation resistance.

[0025] On the other hand, the present application provides a method for preparing a target material, which comprises the steps of raw material mixing-mechanical alloying-sintering in sequence. The target material prepared by the method has high purity and dense structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 Schematic diagram of the preparation process of the target material of the present invention;

[0027] Figure 2 TEM photos of the amorphous-coated nanocrystalline structure CrMnFeCoNi alloy film prepared in Example 1 of the present invention, wherein a) is a high-definition transmission photo of the cross section of the amorphous-coated nanocrystalline, and b) is a local magnified photo of the amorphous-coated nanocrystalline;

[0028] Figure 3 A hardness comparison diagram of the amorphous-coated nanocrystalline dual-phase CrMnFeCoNi alloy film prepared in Example 2 of the present invention and the face-centered cubic single-phase CrMnFeCoNi alloy film of the prior art;

[0029] Figure 4 TEM photos of the face-centered cubic nanocrystalline single-phase CrMnFeCoNi alloy film prepared in Example 3 of the present invention, wherein a) is a cross-sectional bright field transmission photo, b) is a diffraction spot, and c) is a high-resolution photo;

[0030] Figure 5This is a creep rate comparison diagram of the amorphous-coated nanocrystalline (d=3.8 nm) dual-phase CrMnFeCoNi alloy film prepared in Example 4 and the face-centered cubic nanocrystalline (d=16 nm) single-phase CrMnFeCoNi alloy film prepared in Example 5. DETAILED DESCRIPTION

[0031] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.

[0032] In view of the problem that it is difficult to prepare an amorphous-coated nanocrystalline dual-phase alloy film in the prior art, the present application provides a target material for preparing an amorphous-coated nanocrystalline alloy film, which can prepare an amorphous-coated nanocrystalline dual-phase alloy film by using a target material with a specific ratio, so that a nanocrystalline alloy film with a small grain size (d < 10nm) has better mechanical properties. Specifically, an embodiment of the present invention discloses a target material for preparing an amorphous-coated nanocrystalline alloy film, which includes, in atomic percentage, Cr: 12-25%, Mn: 16-30%, Fe: 10-23%, Co: 9-22%, Ni: 10-26%, and the atomic percentages of Cr, Mn, Fe, Co and Ni are not equal to each other.

[0033] The target material provided in the present application is a target material with a high entropy alloy component, which includes Cr, Mn, Fe, Co and Ni. Furthermore, the atomic percentages of the above elements are different, that is, the target material is not a target material with an equal atomic ratio; wherein the Cr content is 12-25%, specifically, the Cr content is 15-20%; by way of example, the Cr content in the present application is 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24% or 25%.

[0034] The content of Mn is 16-30%, specifically, the content of Mn is 18-25%; for example, the content of Mn in the present application is 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29% or 30%.

[0035] The content of Fe is 10-23%, specifically, the content of Fe is 12-22%; for example, the content of Fe in the present application is 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22% or 23%.

[0036] The Co content is 9-22%, specifically, the Co content is 11-20%; for example, the Co content in this application is 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, and 22%.

[0037] The Ni content is 10-26%, specifically, the Ni content is 12-24%; for example, the Ni content in the present application is 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25% or 26%.

[0038] Furthermore, the present application also provides a method for preparing the target material, comprising the following steps:

[0039] Cr, Mn, Fe, Co and Ni are mixed according to atomic percentage ratio and then mechanically alloyed to obtain alloy powder;

[0040] The alloy powder is sintered to obtain a target material.

[0041] In the above preparation process, alloy powder is first prepared. Specifically, the preparation method of the alloy powder includes washing-drying-mixing in sequence, and the specific steps are as follows:

[0042] Cleaning - clean the mixed powder prepared according to atomic percentage using alcohol in an ultrasonic cleaning machine for 20 to 40 minutes;

[0043] Drying: Place the cleaned powder in a vacuum drying oven for drying at a vacuum degree of 1×10 -4 Pa~1×10 -5 Pa, temperature selection 60℃~100℃, drying time 3h~8h;

[0044] Mixing: The dried powder is placed in a planetary ball mill for ball milling to obtain CrMnFeCoNi alloy powder.

[0045] In the above-mentioned cleaning step, the cleaning time is 22 to 30 minutes; in the above-mentioned drying step, the temperature is 70 to 80° C., and the drying time is 4 to 6 hours.

[0046] The present application then sintered the alloy powder obtained above to obtain a target material, wherein the sintering includes pre-pressing and sintering performed in sequence, and the specific steps are as follows:

[0047] Pre-pressing - a layer of graphite paper is lined inside the target mold to prevent it from sticking to the inner wall during sintering. Then the alloy powder is placed in the graphite mold and finally placed on a small hydraulic press for pre-pressing.

[0048] Sintering: Place the mold into a spark plasma sintering furnace chamber for sintering to obtain a target material.

[0049] In the pre-pressing step, the pre-pressing pressure is 10MPa to 20MPa and the time is 1 to 5h. In the sintering step, the vacuum degree in the furnace chamber during sintering is 8×10 -4 Pa~5×10 -5 Pa, specifically, the vacuum degree is 1×10 -5 Pa~4×10 -5 Pa; the sintering pressure is 20-50MPa, specifically, the sintering pressure is 30-40MPa; the sintering temperature is 600-1000°C, specifically, the sintering temperature is 700-900°C; the heating and cooling rates of the sintering are 40-80°C / min, specifically, the heating and cooling rates of the sintering are 50-70°C / min; the sintering insulation time is 10min-25min, specifically, the sintering insulation time is 15-20min.

[0050] The present application also provides a method for preparing an amorphous-coated nanocrystalline alloy film, comprising:

[0051] The target material is magnetron sputtered on the substrate to obtain an amorphous-coated nanocrystalline alloy film;

[0052] The target material is the target material described in the above scheme or the target material prepared by the preparation method.

[0053] In the process of preparing the alloy film, the above-mentioned target material of the present application is used as a sputtering target material to obtain an amorphous-coated nanocrystalline dual-phase alloy film.

[0054] In the above process, the substrate is a substrate well known to those skilled in the art. In a specific embodiment, the substrate is single crystal silicon. The magnetron sputtering can be performed in an intermittent magnetron sputtering manner. The power supply of the magnetron sputtering is a radio frequency power supply with a power of 80W to 120W, a single sputtering time of 10min to 20min, and an interval of 5min to 10min between two sputtering processes. Specifically, the power is 90 to 100W, a single sputtering time of 12 to 18min, and a gap of 6 to 8min between two sputtering processes. During the sputtering process, a bias voltage may be added or not. When a bias voltage is added, the bias voltage is 60 to 100V, and specifically, the bias voltage is 70 to 80V. The sputtering gas is argon gas with a purity of ≥99.999%, and the pressure in the sputtering chamber of the sputtering is 0.1 to 1Pa, and specifically, the pressure is 0.3 to 0.8Pa.

[0055] The thickness of the amorphous-coated nanocrystalline alloy film prepared in the present application is 500nm-1μm. Specifically, the thickness of the amorphous-coated nanocrystalline alloy film is 0.6-0.8μm; the thickness of the amorphous layer is 1nm-3nm, and the grain size is <10nm.

[0056] The CrMnFeCoNi high entropy alloy target prepared in the present application has a dense structure and can be deposited by magnetron sputtering to prepare an amorphous-coated nanocrystalline two-phase alloy film; the amorphous-coated nanocrystalline high entropy alloy film prepared by this target has a strength of up to 8.95 GPa at 1 μm, which is significantly higher than other high entropy alloy films, and has excellent creep deformation resistance; the preparation process of the amorphous-coated nanocrystalline alloy film is simple and environmentally friendly.

[0057] In order to further understand the present invention, the target material for preparing amorphous-coated nanocrystalline alloy film, its preparation method and application provided by the present invention are described in detail below in combination with embodiments. The protection scope of the present invention is not limited by the following embodiments.

[0058] Size Cr 18 Mn 30 Fe 22 Co 20 Ni 10 The preparation process of alloy target is as follows: Figure 1 The specific steps are as follows:

[0059] (1) Alloy raw materials: Cr, Mn, Fe, Co and Ni powders with purity ≥ 99.999%;

[0060] (2) Ingredients: Cr 18%, Mn 30%, Fe 22%, Co 20%, Ni 10% in atomic percentage, 200 g of ingredients were added to obtain a mixed powder;

[0061] (3) Mechanical alloying:

[0062] Cleaning: Clean the prepared mixed powder with alcohol in an ultrasonic cleaning machine for 30 minutes;

[0063] Drying - Put the cleaned powder into a vacuum drying oven for drying, the vacuum degree is 1×10 -4 Pa, temperature is 80℃, drying time is 6h;

[0064] Mixing: Put the dried powder into a planetary ball mill for mechanical alloying to obtain CrMnFeCoNi alloy powder;

[0065] (4) Sintering:

[0066] Pre-pressing - line the target mold with a layer of graphite paper to prevent sticking to the inner wall during sintering, then place the mixed powder in the graphite mold, and finally put it into a small hydraulic press for pre-pressing;

[0067] Sintering: Place the mold into the spark plasma sintering furnace chamber. When the vacuum degree in the furnace chamber reaches 1×10 -5 Pa; sintering was carried out at a sintering pressure of 20 MPa, a sintering temperature of 1000°C, a heating and cooling rate of 40°C / min, and a holding time of 25 min to obtain a CrMnFeCoNi alloy target.

[0068] Example 1

[0069] The Cr 18 Mn 30 Fe 22 Co 20 Ni 10 The alloy target is used as the sputtering target, and the purity of the target is greater than 99.95%. A radio frequency power supply is selected, the preparation power is 120W, and the bias voltage is 80V. The single sputtering preparation time is 20min, and the cycle is repeated 12 times, a total of 4h, with an interval of 5min between two preparation processes, to prepare a high entropy alloy film with a thickness of about 1μm.

[0070] like Figure 2 As shown, Figure 2 TEM photos of the amorphous-coated nanocrystalline CrMnFeCoNi alloy film prepared in this embodiment, wherein a) is a high-definition transmission photo of the amorphous-coated nanocrystals, and b) is a local magnified photo of the amorphous-coated nanocrystals, from which disordered amorphous phase (such as the lower right inset in b) and face-centered cubic nanocrystal phase (such as the upper right inset in b) can be seen.

[0071] Example 2

[0072] The Cr 18 Mn 30 Fe 22 Co 20 Ni 10 The alloy target is used as the sputtering target, and the purity of the target is greater than 99.95%. A radio frequency power supply is selected, the preparation power is 100W, and a bias voltage of 60V is added at the same time. The single sputtering preparation time is 20min, and the cycle is repeated 9 times, a total of 3h, with an interval of 10min between two preparation processes, to prepare an amorphous-coated nanocrystalline two-phase CrMnFeCoNi alloy film with a thickness of 0.8μm.

[0073] like Figure 3 As shown, Figure 3This is a comparison chart of the hardness of the amorphous-coated nanocrystalline dual-phase CrMnFeCoNi alloy film prepared in this embodiment and the face-centered cubic single-phase CrMnFeCoNi alloy film with equal atomic ratio in the prior art. Figure 3 In the table, Liu represents the hardness of the CrMnFeCoNi alloy film with equal atomic ratio at a certain particle size, Lee represents the hardness of the CrMnFeCoNi alloy film with equal atomic ratio at a certain particle size, Shahmir represents the hardness of the CrMnFeCoNi alloy film with equal atomic ratio at a certain particle size, Heczel represents the hardness of the CrMnFeCoNi alloy film with equal atomic ratio at a certain particle size, Schuh represents the hardness of the CrMnFeCoNi alloy film with equal atomic ratio at a certain particle size, Dual-phase represents the hardness of the amorphous-coated nanocrystalline dual-phase CrMnFeCoNi alloy film with a certain particle size prepared in this embodiment, and Monophase represents the hardness of the single-phase Cr 18 Mn 30 Fe 22 Co 20 Ni 10 The hardness of the alloy film at a specific particle size (the preparation methods of the above groups are different); Figure 3 It can be seen that the hardness of the film prepared in the present application is higher than the hardness of almost all single-phase CrMnFeCoNi alloy films known in the prior art.

[0074] Example 3

[0075] The purchased equiatomic ratio CrMnFeCoNi alloy target was used as the sputtering target, and the purity of the target was greater than 99.99%. A radio frequency power supply was selected, the preparation power was 120W, and a bias voltage of 80V was applied at the same time. The single sputtering preparation time was 20min, and the cycle was repeated 12 times, a total of 4h, with an interval of 5min between two preparation processes, to prepare a face-centered cubic nanocrystalline single-phase CrMnFeCoNi high-entropy alloy film with a thickness of about 1μm.

[0076] like Figure 4 As shown, Figure 4 TEM photos of the face-centered cubic nanocrystalline single-phase CrMnFeCoNi alloy film prepared in this embodiment, wherein a) is a cross-sectional bright field transmission photo, b) is a diffraction spot, and c) is a high-resolution photo. Figure 4 Only the nanocrystalline grain boundaries can be seen.

[0077] Example 4

[0078] Size Cr 16 Mn 28 Fe 22 Co 20 Ni 14 The preparation process of alloy target is as follows: Figure 1 The specific steps are as follows:

[0079] (1) Alloy raw materials: Cr, Mn, Fe, Co and Ni powders with purity ≥ 99.999%;

[0080] (2) Ingredients: Cr 16%, Mn 28%, Fe 22%, Co 20%, Ni 14% in atomic percentage, 200 g of ingredients were added to obtain a mixed powder;

[0081] (3) Mechanical alloying:

[0082] Cleaning: Clean the prepared mixed powder with alcohol in an ultrasonic cleaning machine for 30 minutes;

[0083] Drying - Put the cleaned powder into a vacuum drying oven for drying, the vacuum degree is 1×10 -4 Pa, temperature is 80℃, drying time is 6h;

[0084] Mixing: Put the dried powder into a planetary ball mill for mechanical alloying to obtain CrMnFeCoNi alloy powder;

[0085] (4) Sintering:

[0086] Pre-pressing - line the target mold with a layer of graphite paper to prevent sticking to the inner wall during sintering, then place the mixed powder in the graphite mold, and finally put it into a small hydraulic press for pre-pressing;

[0087] Sintering: Place the mold into the spark plasma sintering furnace chamber. When the vacuum degree in the furnace chamber reaches 1×10 -5 Pa; sintering was performed at a sintering pressure of 20 MPa, a sintering temperature of 1000°C, a heating and cooling rate of 40°C / min, and a holding time of 25 min to obtain a CrMnFeCoNi alloy target. 16 Mn 28 Fe 22 Co 20 Ni 14 The alloy target is used as the sputtering target, and the purity of the target is greater than 99.95%. A radio frequency power supply is selected, the preparation power is 150W, no bias is added, the single sputtering preparation time is 15 minutes, and the cycle is repeated 8 times, a total of 2 hours, with an interval of 5 minutes between two preparation processes, to prepare an amorphous-coated nanocrystalline two-phase alloy film with a thickness of about 0.5μm.

[0088] Example 5

[0089] The purchased equiatomic ratio CrMnFeCoNi alloy target was used as the sputtering target, and the purity of the target was greater than 99.99%. A radio frequency power supply was selected, the preparation power was 150W, no bias was added, the single sputtering preparation time was 15 minutes, and 8 cycles were performed, a total of 2 hours, with an interval of 5 minutes between two preparation processes, to prepare a face-centered cubic nanocrystalline single-phase CrMnFeCoNi alloy film with a thickness of about 0.5μm.

[0090] like Figure 5 As shown, Figure 5 The creep rate comparison diagram of the amorphous-coated nanocrystalline (d=3.8 nm) dual-phase CrMnFeCoNi alloy film prepared in Example 4 and the face-centered cubic nanocrystalline (d=16 nm) single-phase CrMnFeCoNi alloy film prepared in Example 5 is shown in FIG. Figure 5 It can be seen that the creep deformation resistance of the amorphous-coated nanocrystalline dual-phase alloy film prepared in Example 4 is better than that of the face-centered cubic nanocrystalline single-phase alloy film prepared in Example 5.

[0091] The above embodiments are only used to help understand the method and core idea of ​​the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

[0092] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A target material for preparing an amorphous-coated nanocrystalline alloy film, comprising, in atomic percentage, Cr: 12-25%, Mn: 16-30%, Fe: 10-23%, Co: 9-22%, Ni: 10-26%, and the atomic percentages of Cr, Mn, Fe, Co and Ni are not equal to each other.

2. The target material according to claim 1, characterized in that The Cr content is 15-20%, and the Mn content is 18-25%.

3. The target material according to claim 1, characterized in that The Fe content is 12 to 22%, the Co content is 11 to 20%, and the Ni content is 12 to 24%.

4. The method for preparing the target material according to claim 1, comprising the following steps: Cr, Mn, Fe, Co and Ni are mixed according to atomic percentage ratio and then mechanically alloyed to obtain alloy powder; The alloy powder is sintered to obtain a target material.

5. The preparation method according to claim 4, characterized in that: The preparation process of the alloy powder is specifically as follows: Ultrasonic cleaning of the mixed powder prepared according to atomic percentage ratio for 20 to 40 minutes; The cleaned powder is dried at a vacuum degree of 1×10 -4 Pa~1×10 -5 Pa, the drying temperature is 60-100°C, and the drying time is 3-8h; The dried powder is ball-milled to obtain alloy powder.

6. The preparation method according to claim 4, characterized in that: The steps of obtaining the target material are specifically as follows: Pre-pressing the alloy powder to obtain an initial target material; The initial target material is subjected to spark plasma sintering to obtain a target material.

7. The preparation method according to claim 6, characterized in that: The pre-pressing pressure is 10MPa-20MPa, and the pre-pressing time is 1-5h.

8. The preparation method according to claim 6, characterized in that: The spark plasma sintering was carried out at 8×10 -4 Pa~5×10 -5 The spark plasma sintering is carried out under a vacuum degree of Pa, the pressure of the spark plasma sintering is 20-50MPa, the temperature of the spark plasma sintering is 600°C-1000°C, the heating rate before sintering and the cooling rate after sintering are 40°C / min-80°C / min respectively, and the sintering holding time is 10min-25min.

9. A method for preparing an amorphous-coated nanocrystalline alloy film, comprising: The target material is magnetron sputtered on the substrate to obtain an amorphous-coated nanocrystalline alloy film; The target material is the target material according to any one of claims 1 to 3 or the target material prepared by the preparation method according to any one of claims 4 to 8.

10. The preparation method according to claim 9, characterized in that: The substrate is single crystal silicon; the magnetron sputtering is intermittent magnetron sputtering, the power supply is a radio frequency power supply, the power is 80W to 120W, the single sputtering time is 10min to 20min, and the interval between two sputtering processes is 5min to 10min; the sputtering gas is argon gas with a purity of ≥99.999%, and the pressure in the sputtering chamber is 0.1Pa to 1Pa; the thickness of the alloy film is 500nm to 1μm, of which the thickness of the amorphous layer is 1nm to 3nm, and the grain size is less than 10nm.