High-carbon 8Mn medium-manganese steel warm-rolled plate as well as preparation method and application thereof

By increasing the content of C element and warm rolling process, combined with tempering heat treatment, the problem of insufficient mechanical properties of the existing technology of high-carbon 8Mn medium-manganese steel is solved, and a high-strength, high-carbon 8Mn medium-manganese steel temperature rolling plate is prepared to meet the needs of automotive materials performance requirements.

CN118932241APending Publication Date: 2024-11-12WUAN BEIKE ADVANCED STEEL TECHNOLOGY SERVICE CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411204135.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art is difficult to prepare high-strength high-carbon 8Mn medium-manganese steel temperature rolled plates through simple and low-cost processes, and its mechanical properties are largely different from those of 9-12Mn medium-manganese steel, making it difficult to meet the material properties of automotive parts. Require.

Method used

By increasing the content of element C and combining warm rolling and post-rolling heat treatment, a high-carbon 8Mn medium-manganese steel temperature-rolling plate was developed. The steps of vacuum smelting, forging, hot rolling, warm rolling and tempering were used to form high-strength and Medium manganese steel showing continuous yielding behavior.

Benefits of technology

It has achieved the significant improvement of the strength and mechanical properties of medium manganese steel while ensuring simple operation, low cost and high efficiency. It is suitable for automotive materials, with a yield strength of 766-789MPa, a tensile strength of 1570-1685MPa, and an elongation of 20.6-21.3%, the strong plastic accumulation is 33.4-34.7 GPa%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932241A_ABST
    Figure CN118932241A_ABST
Patent Text Reader

Abstract

The embodiment of the invention relates to a high-carbon 8Mn medium-manganese steel warm-rolled plate as well as a preparation method and application thereof, and belongs to the technical field of third-generation ultrahigh-strength steel for automobiles. The preparation method of the high-carbon 8Mn medium-manganese steel warm-rolled plate comprises the following steps: (1) smelting: smelting and casting a steel ingot in a vacuum environment to obtain a cannonball-shaped cast ingot; (2) forging: forging the cast ingot into a plate blank, and then air-cooling the plate blank to room temperature; (3) hot rolling is conducted, specifically, the plate blank is subjected to six-pass hot rolling to obtain a thin plate, and then the thin plate is subjected to water quenching to the room temperature; (4) warm rolling is conducted, specifically, the thin plate is heated and subjected to six-pass warm rolling after being subjected to heat preservation for a period of time, and then the thin plate is subjected to water quenching to the room temperature; and (5) heat treatment after rolling is conducted, specifically, the thin plate obtained after warm rolling is subjected to tempering treatment, then water quenching is conducted to the room temperature, and the high-carbon 8Mn medium-manganese steel warm-rolled plate is obtained. The yield strength of the high-carbon 8Mn medium manganese steel warm-rolled plate provided by the embodiment of the invention is 766 to 789 MPa, the tensile strength of the high-carbon 8Mn medium manganese steel warm-rolled plate is 1570 to 1685 MPa, the elongation of the high-carbon 8Mn medium manganese steel warm-rolled plate is 20.6 to 21.3 percent, and the product of strength and elongation of the high-carbon 8Mn medium manganese steel warm-rolled plate is 33.4 to 34.7 GPa percent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The embodiments of the present application relate to the technical field of third-generation ultra-high-strength steel for automobiles, and in particular to a high-carbon 8Mn medium manganese steel warm-rolled plate and a preparation method and application thereof. Background Art

[0002] With the continuous increase in the number of cars, energy conservation and emission reduction have received widespread attention. Therefore, lightweighting of automobiles has become a new trend in the development of the industry. As a new generation of high-strength steel for automobiles, medium manganese steel (manganese mass fraction of 3-12%) has gradually been favored by the automotive industry due to its excellent mechanical properties and lightweight potential, and is used to manufacture a variety of key components. The high strength of medium manganese steel mainly comes from the transformation of austenite to martensite. Mn in steel can not only improve the thermodynamic and mechanical stability of austenite at the same time, but also regulate the stacking fault energy. Studies have shown that stacking fault energy is closely related to TRIP and twinning induced plasticity (TWIP) effects. Generally, medium manganese steel with a Mn mass fraction greater than 9% can exhibit a continuous TWIP-TRIP effect during deformation, thereby obtaining significant mechanical properties and increasing the ability to resist fracture. However, Mn is easily deposited on the steel surface during the smelting process, which makes the wettability of the coating worse. In addition, Mn is also prone to segregation at the grain boundary to form a brittle band, resulting in a decrease in the ductility of the steel. Therefore, even though studies have found that 9-12Mn medium manganese steel has good mechanical properties, it is still difficult to apply it industrially.

[0003] For 8Mn medium manganese steel with industrialization potential, its mechanical properties are still far behind those of 9-12Mn medium manganese steel. The reason is that the reduction of Mn content reduces the stability of austenite, resulting in a large number of martensitic phase transformations at the early stage of deformation. Considering that C can also be used as an austenite stabilizing element, appropriately increasing the C content can not only expand the austenite stable phase region, but also form dispersed carbides and intermetallic compounds in the matrix when combined with the lightweight element Al, thereby improving the strength of medium manganese steel through precipitation strengthening.

[0004] Generally, medium manganese steel needs to undergo intercritical heat treatment after rolling to increase the austenite content in the steel. However, the intercritical annealing process tends to improve the plasticity of medium manganese steel, but it is difficult to make it achieve higher strength, and it cannot meet the material performance requirements of materials in different parts of the automobile. After regulating elements such as C and Mn and introducing warm rolling process to ensure the austenite content in steel, intercritical annealing is no longer the only option for post-rolling heat treatment. Tempering, as a conventional heat treatment method, can not only eliminate intergranular residual stress, but also accelerate the diffusion of Mn and C to improve the stability of austenite. In addition, tempering can also accelerate the formation of precipitation phases. Recently, a study prepared 9Mn steel with a strength of 1560MPa and an elongation of 16.8% by hot rolling and tempering process, indicating the feasibility of tempering as an independent heat treatment method to prepare medium manganese steel.

[0005] In summary, under the premise of ensuring simple operation, low cost and high efficiency, how to prepare high-strength and high-carbon 8Mn medium manganese steel warm-rolled plate by tempering instead of intercritical annealing process has very important significance and practical industrial application value. Summary of the invention

[0006] In view of this, the embodiments of the present application provide a high carbon 8Mn medium manganese steel warm-rolled plate and a preparation method and application thereof. By increasing the C element content and combining warm rolling with post-rolling tempering heat treatment, an 8Mn high carbon medium manganese steel with excellent performance, high strength and continuous yield behavior is developed, which can effectively overcome the defects of the above-mentioned prior art.

[0007] The first aspect of the embodiment of the present application provides a method for preparing a high carbon 8Mn medium manganese steel warm-rolled plate, comprising the following steps:

[0008] (1) Melting: Melting and casting the steel ingot under vacuum to obtain a cannonball-shaped ingot;

[0009] (2) Forging: Forging the ingot into a slab, followed by air cooling to room temperature;

[0010] (3) hot rolling: the slab is hot rolled for six passes to obtain a thin plate, which is then water quenched to room temperature;

[0011] (4) Warm rolling: the sheet is heated and kept warm for a period of time, then warm rolled for six times, and then water quenched to room temperature;

[0012] (5) Post-rolling heat treatment: The thin plate after warm rolling is tempered and then water quenched to room temperature to obtain a high carbon 8Mn medium manganese steel warm rolled plate.

[0013] In some embodiments that may include the above embodiments, in step (1), the steel ingot includes the following components in mass percentage: C 1.17%, Mn 8.10%, Al 5.59%, Cu 2.05%, and the rest is Fe and unavoidable impurities.

[0014] In some embodiments that may include the above embodiments, the specific process of step (2) is: heating the ingot to 1200-1250°C, keeping it warm for 2-3 hours, and then forging it into a slab with a cross-section of 100mm×30mm, and then air-cooling it to room temperature.

[0015] In some embodiments that may include the above embodiments, the specific process of step (3) is: heating the slab to 1200-1250°C, keeping it warm for 2-3h, and then performing six hot rolling passes, with the starting rolling temperature being 1150-1250°C, the final rolling temperature being 900°C, and the rolling reduction for each pass being 13-15%, to obtain a thin plate with a thickness of 4mm±0.4mm, which is then water quenched to room temperature.

[0016] In some embodiments that may include the above embodiments, in step (4), the specific process of the six warm rolling passes is: the thin plate is first rolled to a thickness of 3mm±0.3mm in the first three warm rolling passes, and then the thin plate is kept warm again at 650°C for 15 minutes. After the end, the thin plate is finally rolled to a thickness of 2mm±0.2mm in the last three warm rolling passes.

[0017] In some embodiments that may include the above embodiments, in step (4), the heating temperature is 650° C. and the holding time is 15 min.

[0018] In some embodiments that may include the above embodiments, in step (5), the tempering temperature is 500°C and the tempering time is 1 hour. Different from the traditional intercritical annealing treatment, the post-rolling heat treatment temperature of the present application is 500°C and the tempering is 1 hour. Under long-term tempering, the internal elements of the medium manganese steel are redistributed, so that the austenite can more fully undergo the transformation induced plasticity (TRIP) effect during deformation, and the strength of the medium manganese steel is effectively improved while ensuring a certain elongation. The method of the present application is simple to operate, low in cost, high in efficiency, does not require intercritical annealing heat treatment, has a wide range of applications, and is conducive to process production and application.

[0019] The second aspect of the embodiment of the present application also provides a high carbon 8Mn medium manganese steel warm rolled plate, which is prepared by the above method. The high carbon 8Mn medium manganese steel warm rolled plate has a yield strength of 766-789MPa, a tensile strength of 1570-1685MPa, an elongation of 20.6-21.3%, and a strength-ductility product of 33.4-34.7GPa%.

[0020] A third aspect of the embodiments of the present application also provides the use of the above-mentioned high carbon 8Mn medium manganese steel warm-rolled plate in automotive materials.

[0021] Compared with the prior art, the embodiments of the present application have the following beneficial effects:

[0022] Based on 8Mn steel, the present application appropriately increases the C element content, and ensures the appropriate austenite content in the steel through element regulation and warm rolling process, so that the TRIP effect can occur more slowly and fully during the deformation process, significantly improving the mechanical properties of the product; while ensuring simple operation, low cost and high efficiency, the strength of medium manganese steel is effectively improved, and the industrial production and application of medium manganese steel are promoted. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0024] Figure 1 (a) is the engineering stress-strain curve of Example 1 and Comparative Example 1-1 / 2, Figure 1 (b) is the engineering stress-strain curve of Example 1 and Comparative Example 2-1;

[0025] Figure 2 (a) is a graph of austenite content before and after stretching of Example 1 and Comparative Example 1-1 / 2, Figure 2 (b) is a graph of austenite content before and after stretching of Example 1 and Comparative Example 2-1. DETAILED DESCRIPTION

[0026] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0027] The first aspect of the embodiment of the present application provides a method for preparing a high carbon 8Mn medium manganese steel warm-rolled plate, comprising the following steps:

[0028] (1) Melting: Melting and casting a steel ingot (the steel ingot comprises the following components in mass percentage: C 1.17%, Mn 8.10%, Al 5.59%, Cu 2.05%, and the remainder is Fe and inevitable impurities) in a vacuum environment to obtain a cannonball-shaped ingot;

[0029] (2) Forging: The ingot is heated to 1200-1250° C., kept at this temperature for 2-3 hours, and then forged into a slab with a cross section of 100 mm×30 mm, and then air-cooled to room temperature;

[0030] (3) Hot rolling: the slab is heated to 1200-1250°C, kept at this temperature for 2-3 hours, and then hot rolled in six passes, with the starting rolling temperature being 1150-1250°C, the final rolling temperature being 900°C, and the rolling reduction in each pass being 13-15%, to obtain a sheet with a thickness of 4 mm±0.4 mm, which is then water quenched to room temperature;

[0031] (4) Warm rolling: the thin plate is heated to 650°C, kept at this temperature for 15 minutes, and then warm rolled for six times. The first three warm rolling times roll the thin plate to a thickness of 3 mm ± 0.3 mm. The thin plate is then kept at 650°C for 15 minutes again. After that, the last three warm rolling times roll the thin plate to a thickness of 2 mm ± 0.2 mm, and then water quenched to room temperature.

[0032] (5) Post-rolling heat treatment: The thin plate after warm rolling is tempered at a temperature of 500° C. for 1 h, and then water quenched to room temperature to obtain a high carbon 8Mn medium manganese steel warm-rolled plate.

[0033] The second aspect of the embodiment of the present application also provides a high carbon 8Mn medium manganese steel warm rolled plate, which is prepared by the above method, and the high carbon 8Mn medium manganese steel warm rolled plate has a yield strength of 766-789MPa, a tensile strength of 1570-1685MPa, an elongation of 20.6-21.3%, and a strength-plasticity product of 33.4-34.7GPa%.

[0034] The third aspect of the embodiment of the present application also provides the application of the above-mentioned high carbon 8Mn medium manganese steel warm-rolled plate in automobile materials to meet the needs of different automobile parts.

[0035] Unless otherwise specified, the experimental methods used in the examples of this application are all conventional methods.

[0036] In the following examples and comparative examples, unless otherwise specified, all raw materials can be obtained by commercial purchase or conventional methods.

[0037] Example 1

[0038] The method for preparing the high carbon 8Mn medium manganese steel warm rolled plate in this embodiment comprises the following steps:

[0039] The steel ingot (the steel ingot includes the following components in mass percentage: C 1.17%, Mn 8.10%, Al 5.59%, Cu 2.05%, and the rest is Fe and inevitable impurities) is melted and cast in a vacuum environment to obtain a cannonball-shaped ingot; the ingot is heated to 1200°C, kept warm for 2 hours, and then forged into a slab with a cross section of 100 mm×30 mm, and then air-cooled to room temperature; the slab is heated to 1200°C, kept warm for 2 hours, and then hot-rolled for six times, with the starting rolling temperature of 1200°C, the final rolling temperature of 900°C, and the rolling reduction of each time of 14%, to obtain a 4 mm±0.4 mm thick sheet. The plate is then water quenched to room temperature; the hot-rolled plate is heated to 650°C, kept warm for 15 minutes, and then warm-rolled for six times. The first three times the plate is rolled to a thickness of 3mm±0.3mm, and then the plate is kept warm again at 650°C for 15 minutes. After the end, the last three times of warm rolling are carried out to finally roll the plate to a thickness of 2mm±0.2mm, and then water quenched to room temperature; the warm-rolled plate is placed in a furnace for tempering at 500°C for 1h, and then water quenched to room temperature to obtain a finished high-carbon 8Mn medium-manganese steel warm-rolled plate.

[0040] According to GB / T 228-2010 "Room Temperature Tensile Test Method for Metallic Materials", the finished high carbon 8Mn medium manganese steel warm rolled plate was processed into tensile specimens for mechanical property testing. The obtained engineering stress-strain curve is shown in Figure 1 As shown in Figure 2, the austenite content in the steel before and after stretching is as follows: Figure 2 shown.

[0041] Comparative Example 1-1

[0042] The preparation method of the manganese steel warm-rolled plate in this comparative example comprises the following steps:

[0043] Ingot (The ingot includes the following components by mass percentage: C 1.17%, Mn 8.10%, Al 5.59%, Cu2.05%, the rest Fe and inevitable impurities) are melted and casted in a vacuum environment to obtain a shell-shaped ingot; the ingot is heated to 1200°C, kept warm for 2h, and then forged into a slab with a cross section of 100mm×30mm, and then air-cooled to room temperature; the slab is heated to 1200°C, kept warm for 2h, and then hot-rolled for six times, with a starting rolling temperature of 1200°C, a final rolling temperature of 900°C, and a rolling reduction of 14% per time, to obtain a thin plate with a thickness of 4mm±0.4mm, which is then quenched in water to room temperature; the hot-rolled plate is heated to 650°C, kept warm for 15min, and then warm-rolled for six times, the thin plate is first rolled to a thickness of 3mm±0.3mm in the first three times, and then the thin plate is kept warm again at 650°C for 15min, and then warm-rolled for the last three times to finally roll the thin plate to a thickness of 2mm±0.2mm, which is then quenched in water to obtain a medium manganese steel warm-rolled plate.

[0044] According to GB / T 228-2010 "Room Temperature Tensile Test Method for Metallic Materials", the medium manganese steel hot-rolled plate was processed into tensile specimens for mechanical property testing. The obtained engineering stress-strain curve is shown in Figure 1 As shown in (a), the austenite content in the steel before and after stretching is Figure 2 (a) shown.

[0045] Comparative Example 1-2

[0046] The preparation method of the manganese steel warm-rolled plate in this comparative example comprises the following steps:

[0047] The steel ingot (the steel ingot includes the following components in mass percentage: C 1.17%, Mn 8.10%, Al 5.59%, Cu 2.05%, and the rest is Fe and inevitable impurities) is melted and cast in a vacuum environment to obtain a shell-shaped ingot; the ingot is heated to 1200°C, kept warm for 2 hours, and then forged into a slab with a cross section of 100 mm×30 mm, and then air-cooled to room temperature; the slab is heated to 1200°C, kept warm for 2 hours, and then hot-rolled for six times, with the starting rolling temperature of 1200°C, the final rolling temperature of 900°C, and the rolling reduction of each time of 14%, to obtain 4 mm±0.4 mm thick thin plate, and then quench it to room temperature; the hot-rolled plate is heated to 650℃, kept warm for 15 minutes, and then warm-rolled for six times. The thin plate is rolled to 3mm±0.3mm thick in the first three times, and then the thin plate is kept warm again at 650℃ for 15 minutes. After the end, the thin plate is warm-rolled for the last three times to finally roll it to 2mm±0.2mm thick, and then quenched to room temperature; the thin plate is placed in a furnace for intercritical annealing at 700℃ for 15 minutes to obtain a medium manganese steel warm-rolled plate.

[0048] According to GB / T 228-2010 "Room Temperature Tensile Test Method for Metallic Materials", the medium manganese steel hot-rolled plate was processed into tensile specimens for mechanical property testing. The obtained engineering stress-strain curve is shown in Figure 1 As shown in (a), the austenite content in the steel before and after stretching is Figure 2 (a) shown.

[0049] Comparative Example 2-1

[0050] The preparation method of the manganese steel warm-rolled plate in this comparative example comprises the following steps:

[0051] The steel ingot (the steel ingot includes the following components in mass percentage: C 0.53%, Mn 8.25%, Al 5.58%, Cu 2.15%, and the rest is Fe and inevitable impurities) is melted and cast in a vacuum environment to obtain a shell-shaped ingot; the ingot is heated to 1200°C, kept warm for 2 hours, and then forged into a slab with a cross-section of 100 mm×30 mm, and then air-cooled to room temperature; the slab is heated to 1200°C, kept warm for 2 hours, and then hot-rolled for six times, with a starting rolling temperature of 1200°C, a final rolling temperature of 900°C, and a rolling reduction of 14% in each time, to obtain 4 mm±0.4 mm m thick thin plate, and then quench it to room temperature; the hot-rolled plate is heated to 650℃, kept warm for 15min, and then warm-rolled for six times. The thin plate is rolled to 3mm±0.3mm thick in the first three times, and then the thin plate is kept warm again at 650℃ for 15min. After the end, the thin plate is warm-rolled for the last three times to finally roll it to 2mm±0.2mm thick, and then quenched to room temperature; the warm-rolled plate is placed in a furnace for tempering at 500℃ for 1h, and then quenched to room temperature to obtain a medium manganese steel warm-rolled plate.

[0052] According to GB / T 228-2002 "Room Temperature Tensile Test Method for Metallic Materials", the medium manganese steel hot-rolled plate was processed into tensile specimens for mechanical property testing. The obtained engineering stress-strain curve is shown in Figure 1 As shown in (b), the austenite content in the steel before and after stretching is Figure 2 (b) as shown.

[0053] Application Examples

[0054] Table 1 Mechanical properties test results

[0055]

[0056] Compare the engineering stress-strain curves ( Figure 1 ) and mechanical properties (Table 1) show that, compared with Comparative Example 1-1 (high carbon unheat-treated), Comparative Example 1-2 (high carbon intercritical annealing) and Comparative Example 2-1 (low carbon tempering), Example 1 (high carbon tempering) has significantly improved mechanical properties and exhibits excellent strength, with a yield strength of 766-789MPa, a tensile strength of 1570-1685MPa, an elongation of 20.6-21.3%, and a strength-ductility product of 33.4-34.7GPa%. Compared with intercritical annealing warm-rolled plates, the tempering process increases the tensile strength by 65% ​​without significantly losing the strength-ductility product. Figure 2 It shows that the austenite content of Example 1 before stretching is 36.9%, the austenite content after breaking is 12.2%, and the austenite conversion rate before and after the stretching test is 67%, indicating that the product has both austenite content and stability, which meets the needs of contemporary automotive steel.

[0057] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.

Claims

1. A method for preparing high carbon 8Mn medium manganese steel warm rolled plate, It is characterized in that The following steps are involved: (1) Melting: Melting and casting the steel ingot under vacuum to obtain a cannonball-shaped ingot; (2) Forging: Forging the ingot into a slab, followed by air cooling to room temperature; (3) hot rolling: the slab is hot rolled for six passes to obtain a thin plate, which is then water quenched to room temperature; (4) Warm rolling: the sheet is heated and kept warm for a period of time, then warm rolled for six times, and then water quenched to room temperature; (5) Post-rolling heat treatment: The thin plate after warm rolling is tempered and then water quenched to room temperature to obtain a high carbon 8Mn medium manganese steel warm rolled plate.

2. The method for preparing the high carbon 8Mn medium manganese steel warm rolled plate according to claim 1, It is characterized in that In step (1), the steel ingot comprises the following components in mass percentage: C 1.17%, Mn 8.10%, Al 5.59%, Cu 2.05%, and the remainder is Fe and unavoidable impurities.

3. The method for preparing the high carbon 8Mn medium manganese steel warm rolled plate according to claim 1, It is characterized in that The specific process of step (2) is: heating the ingot to 1200-1250° C., keeping it warm for 2-3 hours, forging it into a slab with a cross section of 100 mm×30 mm, and then air cooling it to room temperature.

4. The method for preparing the high carbon 8Mn medium manganese steel warm rolled plate according to claim 1, It is characterized in that The specific process of step (3) is as follows: heating the slab to 1200-1250°C, keeping it warm for 2-3h, and then performing six hot rolling passes, with the starting rolling temperature being 1150-1250°C, the final rolling temperature being 900°C, and the rolling reduction in each pass being 13-15%, to obtain a thin plate with a thickness of 4mm±0.4mm, which is then water quenched to room temperature.

5. The method for preparing the high carbon 8Mn medium manganese steel warm rolled plate according to claim 1, It is characterized in that In step (4), the specific process of the six warm rolling passes is as follows: the first three warm rolling passes first roll the thin plate to a thickness of 3 mm ± 0.3 mm, then the thin plate is kept warm again at 650°C for 15 minutes, and then the last three warm rolling passes are carried out to finally roll the thin plate to a thickness of 2 mm ± 0.2 mm.

6. The method for preparing the high carbon 8Mn medium manganese steel warm rolled plate according to claim 1, It is characterized in that In step (4), the heating temperature is 650° C. and the insulation time is 15 min.

7. The method for preparing the high carbon 8Mn medium manganese steel warm rolled plate according to claim 1, It is characterized in that In step (5), the tempering temperature is 500° C. and the tempering time is 1 h.

8. A high carbon 8Mn medium manganese steel warm rolled plate, It is characterized in that The high carbon 8Mn medium manganese steel warm rolled plate is prepared by the method described in any one of claims 1 to 7, wherein the high carbon 8Mn medium manganese steel warm rolled plate has a yield strength of 766-789MPa, a tensile strength of 1570-1685MPa, an elongation of 20.6-21.3%, and a strength-ductility product of 33.4-34.7GPa%.

9. Use of the high carbon 8Mn medium manganese steel warm rolled plate according to claim 8 in automobile materials.

Citation Information

Cited By

  • 10Mn medium manganese steel plate with high yield strength and high product of strength and elongation and preparation method of 10Mn medium manganese steel plate