Steel plate for nitriding pot and preparation method

By adjusting the component content of the steel plate, increasing Cu and Al, and reducing Cr content, the hidden dangers of Cr migration to iron pots are solved and the problem of insufficient corrosion resistance and corrosion resistance of iron pots is achieved, and the pot materials are also achieved. .

CN118932245APending Publication Date: 2024-11-12HUNAN VALIN LIANYUAN IRON & STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310523503.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The migration of Cr content in existing iron pots during use is not good for human health and lacks corrosion resistance, which leads to the pots that tend to rust during cooking.

Method used

The steel plate components are C0.02%~0.06% by weight, Si≤0.5%, Mn0.1%~0.5%, P≤0.02%, S≤0.006%, Al0.05%~0.15%, Cu1.1 %~4%, Cr≤0.08%, Ni≤0.05%, As≤0.01%, Cd≤0.01%, Pb≤0.01%, the rest are Fe and inevitable inclusions, which improve corrosion resistance by increasing the content of Cu and Al Performance, reduce Cr content, avoid Cr migration, and avoid the formation of MnS inclusions through low S content.

Benefits of technology

On the premise of ensuring corrosion resistance, the content of Cr is reduced, the harm of Cr migration to human health is avoided, and the thickness and corrosion resistance of the nitriding layer are improved, and the service life of the pot is extended.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932245A_ABST
    Figure CN118932245A_ABST
Patent Text Reader

Abstract

The invention relates to a steel plate for a nitriding pot. The steel plate comprises the following components in percentage by weight: 0.02-0.06% of C, less than or equal to 0.5% of Si, 0.1-0.5% of Mn and less than or equal to 0.02% of P, the alloy comprises the following components in percentage by weight: less than or equal to 0.006% of S, 0.05-0.15% of Al, less than or equal to 0.005% of N, 1.1-4% of Cu, less than or equal to 0.08% of Cr, less than or equal to 0.05% of Ni, less than or equal to 0.01% of As, less than or equal to 0.01% of Cd, less than or equal to 0.01% of Pb and the By adopting the steel plate for the nitriding pot, the corrosion resistance of the steel plate is improved by increasing the content of Cu, so that on the premise of ensuring the corrosion resistance, the content of Cr is reduced, migration caused by over-high content of Cr is avoided, and no harm to human body health is ensured. The invention further relates to a preparation method of the steel plate for the nitriding pot.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cookware materials, and in particular to a steel plate for a nitriding cooker and a preparation method thereof. Background Art

[0002] At present, the materials used to make frying pans are mainly aluminum alloy, stainless steel and iron. Aluminum alloy has good heat conduction and is heated evenly, but aluminum is easy to seep out during cooking, which is not good for health for long-term consumption. Stainless steel pans are light, not easy to rust, high temperature resistant and corrosion resistant, but the price is relatively high. Iron pans have the advantages of high temperature resistance and uniform heat conduction, but they are easy to rust.

[0003] Existing iron pans are generally made of low-carbon steel as the base material. In order to improve corrosion resistance, the low-carbon steel plate is generally stamped or spun, and then nitrided, and 0.1% to 1.5% of Cr is added to the base material. Since Cr accounts for a large proportion of the weight, it will migrate during use, which is harmful to human health. Summary of the invention

[0004] Based on this, it is necessary to provide a nitriding pot steel plate and preparation method that can ensure corrosion resistance and will not be harmful to human health in order to address the problem that Cr will migrate during the use of existing iron pots, which is harmful to human health.

[0005] A steel plate for a nitriding pot, the components of which are as follows by weight percentage: C0.02%~0.06%, Si≤0.5%, Mn0.1%~0.5%, P≤0.02%; S≤0.006%, Al0.05%~0.15%, N≤0.005%, Cu1.1%~4%, Cr≤0.08%, Ni≤0.05%, As≤0.01%, Cd≤0.01%, Pb≤0.01%, and the rest are Fe and unavoidable inclusions.

[0006] By using the above-mentioned steel plate for nitriding pot, the corrosion resistance of the steel plate is improved by increasing the Cu content, thereby reducing the Cr content while ensuring the corrosion resistance, avoiding the migration of Cr due to excessive Cr content, and ensuring that it will not be harmful to human health.

[0007] At the same time, the S content in the above-mentioned steel plate for nitriding pot is low, which avoids the formation of a large number of MnS inclusions and indirectly improves the corrosion resistance. Adding a certain amount of Al increases the thickness of the nitriding layer, thereby also improving the corrosion resistance.

[0008] A method for preparing the above-mentioned steel plate for nitriding pot comprises the steps of: S110, smelting and continuous casting of pure steel into slabs; S120, heating the slab; S130, hot rolling the slab; S140, coiling the slab; S150, pickling the slab; S160, cold rolling the slab; S170, annealing the slab; S180, leveling the slab; S190, re-rolling, oiling and dividing the slab into rolls.

[0009] In one embodiment, the heating temperature in step S120 is 1150° C.-1250° C.

[0010] In one embodiment, the final rolling temperature in step S130 is 880°C-930°C.

[0011] In one embodiment, the coiling temperature in step S140 is 660°C to 720°C.

[0012] In one embodiment, the cumulative reduction rate in step S160 is 60% to 80%.

[0013] In one embodiment, in step S170, annealing is performed in a full hydrogen bell furnace, and the annealing temperature is 700° C. to 760° C.

[0014] In one embodiment, the flattening reduction rate in step S180 is 1% to 1.5%. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0016] Figure 1 A flow chart of a method for preparing a steel plate for a nitriding pot provided in one embodiment of the present application. Implementation

[0017] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.

[0018] An embodiment of the present application provides a steel plate for a nitriding pot, the components of which include, by weight percentage: C0.02%~0.06%, Si≤0.5%, Mn0.1%~0.5%, P≤0.02%; S≤0.006%, Al0.05%~0.15%, N≤0.005%, Cu1.1%~4%, Cr≤0.08%, Ni≤0.05%, As≤0.01%, Cd≤0.01%, Pb≤0.01%, and the rest are Fe and unavoidable inclusions.

[0019] For the above components, it is necessary to explain: C is an indispensable strengthening element in steel and can affect the strength and formability of the steel plate. However, too high a content will affect the formability. Therefore, the content of C in this application is controlled within 0.02% to 0.06%.

[0020] Si can improve the strength of the material, but too high a Si content will easily generate iron oxide scale that is difficult to pickle, affecting the surface quality of the steel plate. Therefore, the Si content in this application is controlled to not exceed 0.5%.

[0021] Mn has the same function as Si, which is used to improve material strength and avoid hot brittle quality problems. However, too much Mn will be detrimental to stamping processing, so the content of Mn is controlled within 0.1%~0.5% in this application.

[0022] P can improve the strength of the material, but too much content will cause the material to be cold and brittle, so in this application the P content is controlled not to exceed 0.02%.

[0023] S can improve material strength, but will reduce plastic forming properties, and will also cause hot brittleness, affecting the surface quality of the steel plate. Mn can combine with S to form MnS, which can easily become the starting point of corrosion and perforation, so the S content should be as low as possible. In this application, the S content is controlled to be no more than 0.006%.

[0024] Al is added as a deoxidizer during steelmaking. When the content is less than 0.01%, it will increase the inclusions in the steel and deteriorate the stamping processing performance. In addition, Al has a strong affinity with N during the nitriding process, which is conducive to the formation of a continuous, dense and relatively thick nitriding layer during the nitriding process, thereby improving the pot body's ability to resist rust and perforation. Therefore, the Al content is controlled to be 0.05%~0.15% in this application.

[0025] N can combine with Al to form AlN precipitates. Dispersed AlN particles hinder grain growth, refine grains and significantly increase strength, while reducing formability. At the same time, too high a N content is not conducive to nitriding, so the N content in this application is controlled to be no more than 0.005%.

[0026] Cu can improve corrosion resistance and is one of the main added elements in steel. Cu can also improve antibacterial effects, but excessive content will lead to high costs. Therefore, the Cu content is controlled to 1.1%~4% in this application.

[0027] Cr can improve corrosion resistance, but the nitriding pot is a metal material for food contact. If the Cr content is too high, migration will occur, which is harmful to human health. Therefore, in this application, the Cr content is controlled to not exceed 0.08%.

[0028] Ni can improve corrosion resistance and is also an element used to control Cu embrittlement. It is generally added to steel containing Cu to prevent Cu embrittlement. However, too high a content is also harmful to human health. Therefore, the Ni content in this application is controlled to not exceed 0.05%.

[0029] As, Pb and Cd are all elements that are harmful to human health and their content should be as low as possible. Therefore, in this application, the content of the three is controlled not to exceed 0.01%.

[0030] By using the above-mentioned steel plate for nitriding pot, the corrosion resistance of the steel plate is improved by increasing the Cu content, thereby reducing the Cr content while ensuring the corrosion resistance, avoiding the migration of Cr due to excessive Cr content, and ensuring that it will not be harmful to human health.

[0031] At the same time, the S content in the above-mentioned steel plate for nitriding pot is low, which avoids the formation of a large number of MnS inclusions and indirectly improves the corrosion resistance. Adding a certain amount of Al increases the thickness of the nitriding layer, thereby also improving the corrosion resistance. See also Figure 1 Based on the steel plate for nitriding pot in the above embodiment, the present application also relates to a method for preparing the steel plate for nitriding pot, comprising the steps of: S110, pure steel is smelted and continuously cast into slabs.

[0032] S120, heating the slab.

[0033] Specifically, the slab is heated to 1150°C to 1250°C.

[0034] S130, hot rolling the slab.

[0035] Specifically, the final rolling temperature is 880°C to 930°C.

[0036] It should be explained that the hot rolling final rolling temperature is higher than the austenite zone temperature of Ar3. If the temperature is too high, the scale will be seriously oxidized, making pickling more difficult and affecting the surface quality of the steel plate; if the temperature is too low, mixed crystals will appear when entering the two zones, and snowflake defects will be generated during stamping, affecting the appearance.

[0037] S140, coiling the slab.

[0038] Specifically, the coiling temperature is 660°C to 720°C.

[0039] It should be explained that high coiling temperature is conducive to grain growth, reducing strength and improving formability. However, too high a temperature will cause serious iron oxide scale on the surface of the steel plate, making pickling difficult and affecting the surface quality of the steel plate.

[0040] S150, pickling the slab.

[0041] S160, cold rolling the slab.

[0042] Specifically, the cumulative reduction rate during the cold rolling process is 60% to 80%.

[0043] It needs to be explained that a larger cold rolling deformation can reduce the recrystallization temperature, but too large a deformation will increase the difficulty of rolling.

[0044] S170, annealing the slab.

[0045] Specifically, the annealing method is annealing in a full hydrogen bell annealing furnace, and the annealing temperature is 700° C. to 760° C.

[0046] It should be explained that the purpose of annealing is to eliminate the hardening effect of cold rolling so that the steel plate has excellent plastic forming properties. However, if the annealing temperature is too high, it will cause abnormal grain growth and produce stamping orange peel or raindrop defects.

[0047] S180, leveling the slab.

[0048] Specifically, the leveling reduction rate is 1% to 1.5%.

[0049] It should be explained that the purpose of flattening is to eliminate the yield platform of the steel plate and avoid the tensile strain mark defects during the stamping process. If the flattening elongation is too low, the yield platform of the steel plate cannot be eliminated, while if the flattening elongation is too high, it will cause work hardening and reduce the plastic processing performance of the material.

[0050] S190, re-rolling, oiling and dividing the slab into rolls. The following describes the preparation methods of the steel plate for the nitriding pot in the present application and the steel plate in the comparative example, and compares their usage.

[0051] Table 1 shows the components and weight percentages of the steel plates for nitriding pots in various embodiments of the present application and the components and weight percentages of the steel plates in comparative embodiments (the rest are iron and unavoidable inclusions). Table 1 Example C(%) Si (%) Mn (%) P(%) S(%) Al(%) N(%) Cu (%) Cr(%) Ni (%) 1 0.0433 0.0267 0.25 0.0124 0.0032 0.098 0.0027 3.61 0.028 0.013 2 0.0527 0.0094 0.42 0.0089 0.0041 0.114 0.0017 1.25 0.033 0.016 3 0.0272 0.0405 0.18 0.0154 0.0041 0.149 0.0019 1.57 0.017 0.02 4 0.0484 0.0172 0.2 0.0117 0.0049 0.092 0.0023 2.38 0.035 0.0161 Comparison 1 0.032 0.019 0.154 0.0096 0.0083 0.0351 0.0052 0.027 0.025 0.0203 Comparison 2 0.04 0.004 0.29 0.0085 0.0062 0.046 0.0024 2.4 1.19 0.83 It should be noted that Example 1 also includes As0.0083%, Cd0.0002% and Pb0.0005%, Example 2 also includes As0.005%, Cd0.0006% and Pb0.0007%, Example 3 also includes As0.0062%, Cd0.0003% and Pb0.0002%, and Example 4 also includes As0.0058, Cd0.0003% and Pb0.0006%.

[0052] The preparation process of Example 1 is as follows: the smelted molten steel is continuously cast into slabs; the slabs are heated in a heating furnace and taken out of the heating furnace at 1208°C; the slabs are rough-rolled and then enter the finishing rolling unit, the finishing rolling temperature is 927°C, the coiling temperature is 683°C, and they are rolled into 4.0mm thick hot-rolled coils; the hot-rolled coils are cold-rolled and acid-rolled into 1.4mm thick hard-rolled coils, with a cold rolling reduction rate of 65%; the hard-rolled coils are placed in a hood-type annealing furnace, annealed at 710°C for 8 hours, and after being taken out of the furnace and cooled, they are leveled on a leveling unit with a leveling reduction rate of 1.2%, and the coils are oiled on a rewinding line.

[0053] The preparation process of Example 2 is as follows: the smelted molten steel is continuously cast into a slab; the slab is heated in a heating furnace and taken out of the heating furnace at 1180°C; the slab is rough-rolled and then enters a finishing rolling unit, the finishing rolling temperature is 911°C, the coiling temperature is 704°C, and the slab is rolled into a 4.0 mm thick hot-rolled coil; the hot-rolled coil is converted to cold-rolled and acid-rolled into a 1.2 mm thick hard-rolled coil, and the cold rolling reduction rate is 70%; the hard-rolled coil is placed in a hood-type annealing furnace, annealed at 740°C for 10 hours, and after being cooled out of the furnace, it is leveled on a leveling unit with a leveling reduction rate of 1.4%, and the coils are oiled on a heavy coiling line.

[0054] The preparation process of Example 3 is as follows: the smelted molten steel is continuously cast into slabs; the slabs are heated in a heating furnace and taken out of the heating furnace at 1235°C; the slabs are rough-rolled and then enter the finishing rolling unit, the finishing rolling temperature is 902°C, the coiling temperature is 725°C, and they are rolled into 4.0mm thick hot-rolled coils; the hot-rolled coils are cold-rolled and acid-rolled into 1.5mm thick hard-rolled coils, and the cold rolling reduction rate is 70%; the hard-rolled coils are placed in a hood-type annealing furnace, annealed at 750°C for 10 hours, and after being cooled out of the furnace, they are leveled on a leveling unit with a leveling reduction rate of 1.2%, and the coils are oiled on a heavy coiling line.

[0055] The preparation process of Example 4 is as follows: the smelted molten steel is continuously cast into a slab; the slab is heated in a heating furnace and taken out of the heating furnace at 1173°C; the slab is rough-rolled and then enters a finishing mill, the finishing rolling temperature is 889°C, the coiling temperature is 718°C, and the slab is rolled into a 3.0 mm thick hot-rolled coil; the hot-rolled coil is converted to cold-rolled and acid-rolled into a 1.2 mm thick hard-rolled coil, and the cold rolling reduction rate is 60%; the hard-rolled coil is placed in a hood-type annealing furnace, annealed at 755°C for 15 hours, and after being cooled out of the furnace, it is leveled on a leveling mill with a leveling reduction rate of 1.3%, and the coils are oiled on a heavy coiling line.

[0056] The preparation process of comparative example 1 is as follows: the smelted molten steel is continuously cast into a slab; the slab is heated in a heating furnace and taken out of the heating furnace at 1214°C; the slab is rough-rolled and then enters a finishing rolling unit, the finishing rolling temperature is 896°C, the coiling temperature is 618°C, and the slab is rolled into a 4.5mm thick hot-rolled coil; the hot-rolled coil is converted to cold-rolled and acid-rolled into a 1.4mm thick hard-rolled coil, and the cold-rolling reduction rate is 68.8%; the hard-rolled coil is placed in a hood-type annealing furnace, annealed at 720°C for 9 hours, and after being cooled out of the furnace, it is leveled on a leveling unit with a leveling reduction rate of 1.0%, and the coils are oiled on a heavy coiling line.

[0057] The preparation process of comparative example 2 is as follows: the smelted molten steel is continuously cast into slabs; the slabs are heated in a heating furnace and taken out of the heating furnace at 1215°C; the slabs are rough-rolled and then enter the finishing rolling unit, the finishing rolling temperature is 920°C, the coiling temperature is 670°C, and they are rolled into 3mm thick hot-rolled coils; the hot-rolled coils are cold-rolled and acid-rolled into 0.5mm thick hard-rolled coils, and the cold-rolling reduction rate is 83.3%; the hard-rolled coils are placed in a hood-type annealing furnace, annealed at 680°C for 6 hours, and after being cooled out of the furnace, they are leveled on a leveling unit with a leveling reduction rate of 1.0%, and the coils are oiled on a heavy coiling line.

[0058] Table 2 is a comparison of the yield strength, tensile strength and elongation of the steel plates in the above-mentioned multiple embodiments.

[0059] Table 2 Table 3 is a comparison of the usage of the steel plates in the above-mentioned multiple embodiments.

[0060] Table 3 The nitriding treatment is carried out in a gas nitriding furnace at a nitriding temperature of 650°C for 2 hours.

[0061] The migration detection method refers to the national standard GB-4806.9 "National Food Safety Standard - Metal Materials and Products for Food Contact".

[0062] The presence or absence of rust spots is determined by the anti-rust perforation test method, which involves boiling the test steel plate with a 5% NaCl solution for 3 hours and observing the presence or absence of rust spots.

[0063] Combined with the above test data, it can be seen that by using the components of the steel plate for nitriding pots in this application and the preparation method in this application, the material mechanical properties of the steel plate prepared, such as yield strength, tensile strength and elongation, meet the process of iron pot stamping or spinning.

[0064] Moreover, in the present application, by increasing the content of Cu and controlling the content of S, the corrosion resistance can still be ensured while reducing the content of Cr and Ni, thereby reducing the content of elements such as Cr and Ni that are unhealthy. At the same time, in the present application, by adding a sufficient amount of Al to promote nitriding and form a continuous and relatively thick nitriding layer, the corrosion resistance is further improved. The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0065] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A steel plate for a nitriding pot, characterized in that: The components by weight percentage include: C0.02%~0.06%, Si≤0.5%, Mn0.1%~0.5%, P≤0.02%; S≤0.006%, Al0.05%~0.15%, N≤0.005%, Cu1.1%~4%, Cr≤0.08%, Ni≤0.05%, As≤0.01%, Cd≤0.01%, Pb≤0.01%, and the rest are Fe and unavoidable inclusions.

2. A method for preparing a steel plate for a nitriding pot according to claim 1, characterized in that: Includes steps: S110, smelting and continuous casting of pure steel into slabs; S120, heating the slab; S130, hot rolling the slab; S140, coiling the slab; S150, pickling the slab; S160, cold rolling the slab; S170, annealing the slab; S180, leveling the slab; S190, re-rolling, oiling and dividing the slab into rolls.

3. The method for preparing a steel plate for a nitriding pot according to claim 2, characterized in that: The heating temperature in step S120 is 1150°C to 1250°C.

4. The method for preparing a steel plate for a nitriding pot according to claim 2, characterized in that: The final rolling temperature in step S130 is 880°C to 930°C.

5. The method for preparing a steel plate for a nitriding pot according to claim 2, characterized in that: The coiling temperature in step S140 is 660°C to 720°C.

6. The method for preparing a steel plate for a nitriding pot according to claim 2, characterized in that: In step S160, the cumulative reduction rate is 60% to 80%.

7. The method for preparing a steel plate for a nitriding pot according to claim 2, characterized in that: In step S170, annealing is performed in a full hydrogen bell furnace, and the annealing temperature is 700°C to 760°C.