Cold heading steel wire rod and preparation method and application thereof
By controlling the composition and preparation process of specific elements in the cold heading steel strips, the problem of poor hardenability of large-scale cold heading steel strips is solved, and excellent hardenability and mechanical properties are achieved, meeting the application of 12.9-level fasteners need.
Patent Information
- Application Number
- CN202410870018.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-01
AI Technical Summary
In the prior art, the hardenability and insufficient mechanical properties of large-sized cold heading steel strips are unable to meet the practical application needs.
By designing specific element composition and preparation process, C: 0.25-0.30wt%, Si: 0.15-0.30wt%, Mn: 0.35-0.60wt%, Cr: 0.70-1.00wt%, Ni: 0.21-0.30wt %, Cu≤0.10wt%, Al: 0.015-0.050wt%, N≤0.007wt%, B: 0.0018-0.0030wt%, Ti: 0.020-0.035wt%, Re: 0.01-0.10wt% Combining the method of pre-designed components and smelting, refining, continuous casting and steel rolling processes, the segregation ratio of carbon and chromium elements and the content of other elements are controlled to form excellent hardenability and mechanical properties.
It achieves excellent hardenability and mechanical properties of large-scale cold heading steel strips, meets the application needs of 12.9-level fasteners, and improves the reliability and quality performance of fasteners.
Smart Images

Figure FT_1 
Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cold heading steel, and in particular to a cold heading steel wire rod and a preparation method and application thereof. Background Art
[0002] Cold heading steel is mainly used to produce fasteners such as bolts and nuts, and is widely used in industries such as automobiles, shipbuilding, and engineering machinery. In recent years, with the development of the industry and technological progress, 12.9 grade high-strength fasteners have been increasingly used.
[0003] Traditional 12.9 grade high-strength fastener steel is mostly medium carbon alloy steel, among which medium carbon CrMo cold heading steel is the representative, including grades SCM435, SCM440, ML42CrMo, etc. This type of steel has high carbon and alloy content and poor cold heading forming performance. Spheroidizing annealing must be completed before cold heading. The spheroidizing annealing process is time-consuming and fuel-intensive, which is not conducive to low-carbon environmental protection and energy-saving requirements.
[0004] Compared with alloy cold heading steel, boron-containing cold heading steel has the advantages of good processing performance and low cost. Boron-containing cold heading steel can reduce the carbon content in steel and the content of alloy elements such as Cr and Mo added to improve hardenability while ensuring the hardenability of fasteners. It can replace trace boron and a small amount of alloy to obtain the same strength. It has good plasticity and cold heading performance, can omit or simplify the annealing process of downstream customers, save fastener manufacturing costs, has good development prospects, and is the development trend of energy-saving cold heading steel in the future. At present, some manufacturers can produce annealing-free or simplified annealing boron steel wire for the production and manufacturing of 12.9 grade fasteners.
[0005] With the development of economy, the demand for large-scale 12.9 grade fastener steel in large-scale projects, bridges, mechanical equipment, etc. is growing. For large-scale fastener steel, hardenability has become a crucial factor to measure its performance, directly affecting the final organization and performance of the fastener. Due to the large size of large-scale wire rods, its hardenability is often difficult to meet the use requirements.
[0006] The currently disclosed cold heading steel preparation process cannot guarantee the hardenability of large-sized wire rods, and the mechanical properties of the wire rods after quenching and tempering treatment cannot meet the requirements of practical applications. Summary of the invention
[0007] Therefore, the technical problem to be solved by the present invention is to overcome the defects in the prior art that large-sized wire rods have poor hardenability and poor mechanical properties after treatment, which cannot meet the requirements of practical applications, thereby providing a cold heading steel wire rod and its preparation method and application.
[0008] The first aspect of the present invention protects a cold heading steel wire rod, wherein, based on the mass of the wire rod, C: 0.25-0.30wt%, Si: 0.15-0.30wt%, Mn: 0.35-0.60wt%, P≤0.020wt%, S≤0.015wt%, Cr: 0.70-1.00wt%, Ni: 0.21-0.30wt%, Cu≤0.10wt%, Al: 0.015-0.050wt%, N≤0.007wt%, B: 0.0018-0.0030wt%, Ti: 0.020-0.035wt%, Re: 0.01-0.10wt%, and the rest are Fe and unavoidable impurities; The cross section of the wire rod is circular, and the ratio (segregation ratio) of the sum of the carbon and chromium contents at the center of the circle to the sum of the carbon and chromium contents at 1 / 2 radius is 1.1-1.2:1.
[0009] In the present invention, the content of the whole element of the wire rod adopts the method of pre-designing the composition, and the specific method is to add alloy according to the pre-design result to fine-tune the element content; and use a carbon-sulfur analyzer, an ICP analyzer or an electron probe analyzer to measure the content of the elements at different positions.
[0010] In the present invention, when the cross section of the wire rod is circular, Figure 1 As shown, the segregation ratio is the ratio of the element content at position a (center of the circle) to that at position b (1 / 2 radius) (or in the same circle as position b).
[0011] In the present invention, each element in the wire rod: C: It plays a role in solid solution strengthening, improving the hardenability and strength of the wire rod after quenching and tempering. However, too high a C content will reduce the plasticity and toughness of the wire rod after quenching and tempering, resulting in poor forming performance of fasteners and increasing the risk of delayed fracture. Taking all factors into consideration, the C content is controlled to be 0.25-0.30wt%.
[0012] Si: It is a deoxidizing element in steel. It improves the strength of the wire rod after quenching and tempering through solid solution strengthening. However, too high Si content will lead to a decrease in the plasticity and toughness of the wire rod after quenching and tempering, which is not conducive to the forming of fasteners. At the same time, it will accelerate the decarburization of steel during the heating process. Taking all factors into consideration, the Si content is controlled to 0.15-0.30wt%.
[0013] Mn: In the present invention, Mn combines with Cr to form an interstitial solid solution, forming cluster strengthening, and improving the strength and hardenability of the wire rod after quenching and tempering. However, too high a Mn content will increase the temper brittleness and reduce the toughness and delayed fracture resistance of the wire rod after quenching and tempering. Taking all factors into consideration, the Mn content is controlled to be 0.35-0.60wt%.
[0014] P and S: Both are impurity elements, which tend to segregate at grain boundaries to form low-strength inclusion phases, resulting in reduced plasticity and toughness of the wire rod after quenching and tempering, and increased delayed fracture sensitivity. Taking all factors into consideration, the P content is controlled to be ≤0.020wt% and the S content is ≤0.015wt%.
[0015] Cr: In the present invention, it combines with Mn to form an interstitial solid solution, forming cluster strengthening, improving the strength and hardenability of the wire rod after quenching and tempering, and can form chromium-containing carbides with C to improve the tempering softening resistance and delayed fracture resistance of the wire rod after quenching and tempering. However, too high a Cr content will lead to a high strength of the wire rod after quenching and tempering and deteriorate the fastener forming performance, reducing the plasticity of the wire rod after quenching and tempering. Taking all factors into consideration, the Cr content is controlled to be 0.70-1.00wt%.
[0016] Ni: Improves the strength of the wire rod after quenching and tempering through solid solution strengthening, enhances hardenability, and reduces the tough-to-brittle transition temperature. However, too high a Ni content will increase the cost of the wire rod after quenching and tempering. Considering all factors, the Ni content is controlled to be 0.21-0.30wt%.
[0017] Cu: It is a residual element in the present invention, which will cause grain boundary embrittlement, increase crack sensitivity, and reduce delayed fracture resistance. The Cu content is controlled to be ≤0.10wt%.
[0018] Al: It is a strong deoxidizing element, which can improve the oxidation resistance of the wire rod after quenching and tempering, refine the grains, and improve the strength and toughness of the wire rod after quenching and tempering. However, excessive Al will increase the number of coarse carbonitride inclusions and reduce the delayed fracture resistance of the wire rod after quenching and tempering. Taking all factors into consideration, the Al content is controlled to be 0.015-0.050wt%.
[0019] N: It has a solid solution strengthening effect, but excessive N will cause aging brittleness of the steel, reduce the plasticity and bolt forming properties of the wire rod after quenching and tempering, and control the N content to ≤0.007wt%.
[0020] B: It can improve the hardenability and delayed fracture resistance of the wire rod after quenching and tempering, but excessive B will lead to a decrease in the toughness of the wire rod after quenching and tempering. Taking all factors into consideration, the B content is controlled to be 0.0018-0.0030wt%.
[0021] Ti: It mainly plays a role in nitrogen fixation to ensure the hardenability of boron, but too high Ti will increase the number of inclusions in the steel, forming fatigue crack sources and causing the deterioration of bolt forming performance. Considering the N content in the steel and the nitrogen fixation effects of Al and Si, the Ti content is controlled to be 0.020-0.035wt%.
[0022] Re: In order to reduce the segregation of harmful elements such as P and S and impurity elements at the grain boundary, change the composition, morphology, distribution, etc. of inclusions in the steel, improve the low-temperature toughness and fatigue performance of the wire rod after quenching and tempering, reduce temper brittleness, and refine the grain size. Considering all factors, the Re content is controlled to be 0.01-0.10wt%.
[0023] According to the present invention, in addition to the above elements, the remainder of the wire rod is Fe and inevitable impurities.
[0024] According to the present invention, the diameter of the wire rod is 20-40 mm.
[0025] In the present invention, Cr and Mn elements form interstitial solid solutions in the steel, and the formation of clusters can further improve the tensile strength and hardenability of the wire rod after the boron-containing cold heading and tempering treatment. According to relevant experimental studies, the content of the Cr element and the content of the Mn element are controlled to satisfy the formula Cr / Mn=1.5-2.0:1.
[0026] In the present invention, the Ni element, the Ti element and the Al element will combine to form a nano-precipitated phase, further improving the strength of the wire rod and forming a strong hydrogen trap, thereby improving the delayed fracture resistance of the wire rod after quenching and tempering. According to relevant experimental studies, the content of the Ni element, the content of the Ti element and the content of the Al element are controlled to satisfy the formula Ni / (Ti+Al)=3.5-5:1.
[0027] In the present invention, based on the contribution of each alloy element to the hardenability of boron-containing cold heading steel, comprehensive consideration is taken, and in order to meet the hardenability of large-size wire rods, the content of the C element, the content of the Cr element, the content of the Mn element, the content of the Ni element, and the content of the B element are controlled to satisfy the formula (35×C+13×Cr+10×Mn+3×Ni+8000×B)×100≥43.
[0028] The second aspect of the present invention protects a method for preparing the aforementioned cold heading steel wire rod, wherein the preparation method comprises the following steps: The molten iron is smelted, refined, continuously cast and rolled to obtain wire rods; Among them, during continuous casting, the superheat of molten steel in the tundish is 30-40°C, and the drawing speed for billet straightening is 2.5-2.7m / min.
[0029] According to the present invention, the smelting is converter smelting, and the refining is LF refining.
[0030] Converter smelting: molten iron enters the converter for oxygen blowing smelting. The C in the molten steel at the end of converter smelting is 0.08-0.20wt%, P≤0.015wt%, and the tapping temperature at the end of converter smelting is 1620-1660℃. After 25-30% of the steel is tapped, aluminum ingots, ferrosilicon, low carbon ferromanganese, high carbon ferrochrome, ferronickel and lime are added in sequence for deoxidation and alloying. During the tapping process, argon is blown from the bottom of the ladle. The argon blowing flow rate is controlled at 650-800L / min in the early and middle stages of tapping. After 70-80% of the steel is tapped, the argon blowing flow rate is controlled at 300-450L / min.
[0031] LF refining: After the converter molten steel enters the LF station, lime and fluorite are added in sequence to adjust the white slag. After the white slag is refined for 5-10 minutes, titanium iron, boron iron and rare earth iron alloy are added in sequence for alloying, and the basicity of the final refined slag is controlled to be 3.5-5. During the alloying period, the argon flow rate of the bottom blowing of the ladle is 300-450L / min; then the temperature is raised to 1550-1565℃, and samples are taken for chemical composition detection. According to the test results, alloys are added to fine-tune the chemical composition. During the chemical composition fine-tuning period, the argon flow rate of the bottom blowing of the ladle is 150-300L / min; before soft stirring, calcium wire is fed into the molten steel, the amount of calcium wire added is 0.8-1.0m / t, the calcium wire feeding speed is 170-200m / min, the soft stirring time is 25-35min, and the bottom blowing argon flow rate is 30-80L / min during soft stirring; the steel tapping temperature at the end point of LF refining is controlled to be 1570-1595℃.
[0032] Continuous casting: LF is refined and then cast. During the continuous casting process, argon seal is used for long water inlet of large ladle, alkaline tundish covering agent and immersed water inlet are used for full protection casting. Low carbon steel protective slag is used for protective slag. The superheat of molten steel in tundish is controlled at 30-40℃, the liquid level of crystallizer is 80-85% of the height of crystallizer, the liquid level fluctuation range is within ±3%, the electromagnetic stirring current of crystallizer is 350-500A, the stirring frequency is 1.5-2Hz, the secondary cooling water ratio is controlled at 0.8-1.0L / kg, and the drawing speed of billet straightening is 2.5-2.7m / min.
[0033] In the present invention, after continuous casting, a cast billet is obtained, and the cross-sectional size of the cast billet is mainly determined by the equipment. When the cross-sectional area of the cast billet is circular, the diameter of the circle is 140-160 mm; when the cross-sectional area of the cast billet is square, the side length of the square is 140-160 mm. In the present invention, the cross-sectional area of the wire rod obtained after the cast billet is rolled is circular.
[0034] According to the present invention, the steel rolling includes heating, high-speed wire rolling and controlled cooling.
[0035] The details are as follows: Heating: The heating process includes a heating section and a soaking section. The temperature of the heating section is 1050-1090°C, and the holding time is 30-40 minutes; the temperature of the soaking section is 1080-1120°C, and the holding time is 15-25 minutes. The air-fuel ratio of the heating furnace is controlled to be 0.60-0.65:1. By setting the above-mentioned heating section temperature and the heating section holding time, the alloy elements can be further dissolved in the austenite to avoid cracks caused by excessive temperature stress during the rolling process. At the same time, the rolling production rhythm is improved, the uniformity of heating is ensured, oxidation and decarburization are minimized, and defects such as overheating and overburning are prevented. By setting the above-mentioned soaking section temperature and the soaking section holding time, the temperature difference between the surface and the core of the wire rod can be further reduced, the steel temperature can be uniformed, and the internal structure and performance of the billet can be improved.
[0036] High-speed wire rolling: Control the starting rolling temperature to 960-1000°C, the finishing rolling entrance temperature to 880-910°C, and perform three-stage water tank cooling, with the three-stage water tank flow ratio being (5±0.5):(3±0.5):(2±0.5). By setting the above starting rolling temperature and finishing rolling temperature, the brittle temperature range of the wire rod of the present invention can be further avoided, so that the wire rod has good structure and performance. By reasonably allocating the water volume in the water tank, the temperature difference between the surface and the core of the wire rod can be reduced, and the uniformity of the wire rod structure can be improved.
[0037] Controlled cooling: Control the coiling temperature to 840-870℃, turn on the first 1-2 fans, control the fan air volume to 70-100%, and turn off all other fans and insulation covers. Through the above controlled cooling process settings, the uniformity of the wire rod microstructure can be further controlled to form fine equiaxed ferrite and pearlite structures.
[0038] The third aspect of the present invention protects the use of the aforementioned wire rod or the wire rod obtained by the aforementioned preparation method after quenching and tempering in a 12.9 grade fastener.
[0039] In the present invention, the quenching and tempering treatment is a conventional quenching and tempering treatment, which is first quenched at a temperature of 850-880°C and a quenching and holding time of 30-60 minutes, and then tempered at a temperature of 510-530°C and a tempering and holding time of 80-120 minutes.
[0040] The technical solution of the present invention has the following advantages: 1. The present invention provides a cold heading steel wire rod, wherein, based on the mass of the wire rod, C: 0.25-0.30wt%, Si: 0.15-0.30wt%, Mn: 0.35-0.60wt%, P≤0.020wt%, S≤0.015wt%, Cr: 0.70-1.00wt%, Ni: 0.21-0.30wt%, Cu≤0.10wt%, Al: 0.015-0.050wt%, N≤0.007wt%, B: 0.0018-0.0030wt%, Ti: 0.020-0.035wt%, Re: 0.01-0.10wt%, and the remainder is Fe and unavoidable impurities; the cross section of the wire rod is circular, and the ratio of the sum of the carbon and chromium contents at the center of the circle to the sum of the carbon and chromium contents at 1 / 2 radius is 1.1-1.2:1. The present invention overcomes the technical prejudice about segregation. Different from the prior art which aims to reduce the segregation ratio, the present application controls the sum of carbon and chromium elements in the wire rod to meet a specific segregation ratio, thereby reducing the critical cooling rate for forming martensite in the core of the wire rod and improving the hardenability of the core. This allows the wire rod to have excellent hardenability in the subsequent quenching process, and the treated wire rod has excellent mechanical properties.
[0041] 2. The present invention limits the specific size of the wire rod, which proves that the present invention can be applied to process large-sized wire rods. Although the size is large, it can still be fully hardened and has good hardenability, thereby improving the reliability of the wire rod as a fastener, reducing the risk of failure, and further improving the quality performance of large-sized cold-headed steel wire rods.
[0042] 3. The preparation method of the present invention comprises the following steps: molten iron is smelted, refined and continuously cast to prepare a cast billet, and the cast billet is rolled to obtain a wire rod; wherein, during continuous casting, the superheat of the molten steel in the tundish is 30-40°C, and the drawing speed of the billet straightening is 2.5-2.7 m / min. In the present invention, by controlling a specific superheat and a specific drawing speed of the billet straightening, a certain segregation is deliberately made in the center of the wire rod, so that the critical cooling rate of the formation of martensite in the center is reduced, and the hardenability of the center is improved, so that the treated wire rod has excellent mechanical properties.
[0043] 4. After the tempering treatment, the wire rod obtained by the present invention has excellent hardness and tensile properties, and can meet the application requirements of 12.9 grade fastener steel. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0045] Figure 1 It is a schematic diagram of the cross section of the wire rod according to Example 1 of the present invention.
[0046] Reference numerals: a-center of the circle; b-1 / 2 radius. DETAILED DESCRIPTION
[0047] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0048] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0049] Preparation Example This preparation example provides a cold heading steel ingot and a preparation method thereof, and the specific steps are as follows: Examples 1-10 and Comparative Examples 1-10 were all operated according to this procedure, and the different parameters are shown in Table 1.
[0050] Converter smelting: molten iron enters the converter for oxygen blowing smelting. The C and P contents in the molten steel at the end of converter smelting are controlled as shown in Table 1. The tapping temperature at the end of converter smelting is shown in Table 1. After 25% of the steel is tapped, aluminum ingots, ferrosilicon, low-carbon ferromanganese, high-carbon ferrochrome, ferronickel and lime are added in sequence for deoxidation and alloying. The amount of each component is controlled. During the tapping process, argon is blown from the bottom of the ladle. The argon blowing flow rate is controlled to be 700L / min in the early and middle stages of the tapping. After 75% of the steel is tapped, the argon blowing flow rate is controlled to be 400L / min.
[0051] LF refining: After the converter molten steel enters the LF station, lime and fluorite are added in sequence to adjust the white slag. After the white slag is refined for 8 minutes, titanium iron, boron iron and rare earth iron alloy are added in sequence for alloying. The basicity of the final slag is controlled as shown in Table 1. During the alloying period, the argon flow rate of the bottom of the ladle is 400L / min; then the temperature is raised to 1560℃, and samples are taken for chemical composition detection. According to the test results, alloys are added to fine-tune the chemical composition. During the chemical composition fine-tuning period, the argon flow rate of the bottom of the ladle is 250L / min; before soft stirring, calcium wire is fed into the molten steel, the amount of calcium wire added is 0.8m / t, the calcium wire feeding speed is 180m / min, the soft stirring time is 30min, and the bottom blowing argon flow rate is 60L / min during soft stirring; the tapping temperature at the end of LF refining is controlled as shown in Table 1.
[0052] Continuous casting: LF is refined and then cast. In the continuous casting process, argon seal of long water inlet of large ladle, alkaline tundish covering agent and submerged water inlet are used for full protection casting. Low carbon steel protective slag is used for protective slag. The superheat of molten steel in tundish is controlled as shown in Table 1. The liquid level of crystallizer is 83% of the height of crystallizer, and the liquid level fluctuation range is within ±3%. The electromagnetic stirring current of crystallizer is 350A, the stirring frequency is 1.8Hz, the secondary cooling water volume is controlled to be 0.8L / kg, and the drawing speed of billet straightening is shown in Table 1.
[0053] The ingot is rolled to obtain wire rods, and the rolling process specifically includes heating, high-speed wire rolling, and controlled cooling.
[0054] Heating: The heating process includes a heating section and a soaking section. The temperature of the heating section is 1065°C and the holding time is 35 minutes. The temperature of the soaking section is 1096°C and the holding time is 23 minutes. The air-fuel ratio of the heating furnace is controlled at 0.62:1. By setting the above-mentioned heating section temperature and the heating section holding time, the alloy elements can be further dissolved in the austenite to avoid cracks caused by excessive temperature stress during the rolling process. At the same time, the rolling production rhythm can be improved to ensure the uniformity of heating, minimize oxidation and decarburization, and prevent defects such as overheating and overburning. By setting the above-mentioned soaking section temperature and the soaking section holding time, the temperature difference between the surface and the core of the ingot can be further reduced, the steel temperature can be uniformed, and the internal structure and performance of the ingot can be improved.
[0055] High-speed wire rolling: the start rolling temperature is controlled at 984°C, the finishing rolling inlet temperature is controlled at 891°C, and three-stage water tank cooling is performed. The flow rate of the first stage water tank is 2141L / min, the flow rate of the second stage water tank is 1264L / min, and the flow rate of the third stage water tank is 857L / min. The water tank flow ratio is 4.9:2.9:2. By setting the above-mentioned start rolling temperature and finishing rolling temperature, the brittle temperature range of the wire rod of the present invention can be further avoided, so that the wire rod has good organization and performance. By reasonably allocating the water volume of the water tank, the temperature difference between the surface and the core of the wire rod is reduced, and the uniformity of the wire rod organization is improved.
[0056] Cooling control: The coiling temperature is controlled at 849°C, the first fan is turned on, and the fan air volume is controlled to 80%, the second fan is turned on, and the fan air volume is controlled to 80%, the remaining fans are all turned off, and the insulation covers are all closed to obtain the wire rod.
[0057] Table 1 C content in molten steel / % P content in molten steel / % Steel tapping temperature at the end of converter smelting / ℃ Final slag basicity LF refining end point tapping temperature / ℃ Superheat of molten steel in tundish / ℃ Drawing speed of billet straightening / (m / min) Example 1 0.12 0.012 1635 3.98 1583 32 2.5 Example 2 0.13 0.007 1642 4.22 1592 31 2.6 Example 3 0.18 0.008 1639 4.67 1577 39 2.7 Example 4 0.09 0.01 1651 4.34 1590 35 2.6 Example 5 0.15 0.01 1643 4.51 1582 33 2.5 Example 6 0.12 0.006 1638 4.76 1573 34 2.6 Example 7 0.11 0.01 1657 4.83 1586 35 2.6 Example 8 0.12 0.011 1634 3.62 1587 36 2.5 Example 9 0.14 0.007 1646 4.15 1582 33 2.6 Example 10 0.11 0.009 1641 4.37 1591 34 2.5 Comparative Example 1 0.08 0.01 1625 4.42 1574 37 2.7 Comparative Example 2 0.12 0.008 1646 4.23 1585 36 2.5 Comparative Example 3 0.13 0.01 1635 3.76 1579 35 2.6 Comparative Example 4 0.09 0.011 1648 4.19 1583 32 2.5 Comparative Example 5 0.12 0.01 1637 4.34 1581 35 2.6 Comparative Example 6 0.17 0.01 1628 4.05 1584 34 2.7 Comparative Example 7 0.15 0.011 1647 4.72 1576 35 2.5 Comparative Example 8 0.16 0.01 1639 3.95 1594 38 2.6 Comparative Example 9 0.18 0.011 1649 4.87 1588 32 2.5 Comparative Example 10 0.13 0.009 1634 4.64 1573 35 2.7 The segregation ratio of the total carbon element and chromium element in the wire rod is shown in Table 2.
[0058] Table 2 Segregation ratio Example 1 1.13 Example 2 1.15 Example 3 1.17 Example 4 1.16 Example 5 1.14 Example 6 1.11 Example 7 1.14 Example 8 1.12 Example 9 1.14 Example 10 1.15 Comparative Example 1 1.01 Comparative Example 2 0.99 Comparative Example 3 1.05 Comparative Example 4 1.02 Comparative Example 5 1.03 Comparative Example 6 0.98 Comparative Example 7 1.03 Comparative Example 8 0.97 Comparative Example 9 1.02 Comparative Example 10 1.04 The content of the whole element of the wire rod adopts the method of pre-designed composition. The specific method is to add alloy to fine-tune the element content according to the pre-designed results and test results in Table 3. The specific data of each element in the round wire rod are shown in Table 3.
[0059] Table 3
[0060] Table 3 continued Example 6 Example 7 Example 8 Example 9 Example 10 C 0.25 0.3 0.28 0.27 0.26 Si 0.2 0.22 0.23 0.17 0.26 Mn 0.37 0.59 0.57 0.58 0.53 P 0.008 0.012 0.013 0.009 0.011 S 0.004 0.008 0.009 0.01 0.006 Cr 0.72 0.93 0.98 0.92 0.97 Ni 0.28 0.27 0.23 0.21 0.23 Cu 0.03 0.03 0.02 0.04 0.03 Al 0.033 0.028 0.031 0.029 0.025 N 0.0046 0.0061 0.0058 0.0059 0.0063 B 0.0028 0.0019 0.0022 0.0027 0.002 Ti 0.024 0.032 0.031 0.028 0.035 Re 0.02 0.06 0.08 0.05 0.02 Cr / Mn 1.95 1.58 1.72 1.59 1.83 Ni / (Ti+Al) 4.91 4.50 3.71 3.68 3.83 (35×C+13×Cr+10×Mn+3×Ni+8000×B)×100 45.05 44.50 46.53 49.44 43.70 Table 3 continued Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 C 0.19 0.28 0.27 0.28 0.27 Si 0.25 0.23 0.18 0.25 0.27 Mn 0.5 0.54 0.72 0.46 0.58 P 0.012 0.01 0.012 0.013 0.012 S 0.007 0.005 0.006 0.005 0.007 Cr 0.98 0.53 0.96 1.31 0.74 Ni 0.25 0.22 0.21 0.23 0.24 Cu 0.02 0.03 0.02 0.02 0.02 Al 0.037 0.026 0.032 0.037 0.033 N 0.0054 0.0062 0.0051 0.006 0.0058 B 0.0023 0.0026 0.0021 0.0022 0.0026 Ti 0.027 0.032 0.026 0.023 0.028 Re 0.03 0.04 0.02 0.05 0.04 Cr / Mn 1.96 0.98 1.33 2.85 1.28 Ni / (Ti+Al) 3.91 3.79 3.62 3.83 3.93 (35×C+13×Cr+10×Mn+3×Ni+8000×B)×100 43.54 43.55 46.56 49.72 46.39 Table 3 continued Comparative Example 6 Comparative Example 7 Comparative Example 8 Comparative Example 9 Comparative Example 10 C 0.38 0.26 0.27 0.29 0.28 Si 0.24 0.21 0.26 0.25 0.22 Mn 0.53 0.4 0.49 0.51 0.56 P 0.014 0.013 0.012 0.014 0.011 S 0.005 0.004 0.009 0.006 0.005 Cr 0.97 0.76 0.93 0.94 0.96 Ni 0.25 0.23 0.28 0.25 0.28 Cu 0.03 0.02 0.02 0.02 0.03 Al 0.038 0.041 0.025 0.034 0.045 N 0.0064 0.0049 0.0055 0.0066 0.0052 B 0.0023 0.002 0.0024 0.0022 0.0025 Ti 0.024 0.023 0.052 0.032 0.022 Re 0.06 0.05 0.03 0.07 0.04 Cr / Mn 1.83 1.90 1.90 1.84 1.71 Ni / (Ti+Al) 4.03 3.59 3.64 3.79 4.18 (35×C+13×Cr+10×Mn+3×Ni+8000×B)×100 50.36 39.67 46.48 45.82 48.72 The wire rods of Examples 1-10 and Comparative Examples 1-10 were further subjected to tempering treatment.
[0061] The specific steps of the quenching and tempering treatment are: quenching the wire rod, the quenching temperature is 870°C, the quenching holding time is 40 minutes, the tempering temperature is 530°C, the tempering holding time is 80 minutes, and the quenched and tempered wire rod is obtained.
[0062] The Rockwell hardness (HRC) of the cross section and surface of the wire rod after quenching and tempering was tested in accordance with GB / T 230.1-2018. The specific results are shown in Table 4.
[0063] Table 4
[0064] After tempering treatment, the Rockwell hardness at the center of the cross section of the embodiment is ≥37.5HRC, the Rockwell hardness at the 1 / 2 radius of the cross section is ≥40.8HRC, the Rockwell hardness 2mm near the surface of the cross section is ≥42HRC, and the Rockwell hardness of the wire rod surface is ≥43HRC. It can be seen from the data of the embodiment that the center of the circle also has a higher hardness, indicating that the depth of the hardness value is large, which can prove that the embodiment has a higher hardenability; the cross-sectional hardness difference of the embodiment is ≤5HRC, and the cross-sectional hardness difference of the comparative example is >10HRC. The hardenability of the embodiment is significantly improved compared with the comparative example, and the surface hardness of comparative example 1 and comparative example 2 is <39HRC, and the service life is not as good as that of the embodiment.
[0065] The segregation ratio in the comparative example does not meet the range defined by the present invention, the composition difference between the core of the wire rod and the matrix is small, the hardenability is poor, the hardness of the core obtained is low, and the cross-sectional hardness difference is large. Compared with the comparative example, the embodiment has excellent hardenability, and at the same time has higher strength and excellent delayed fracture resistance, and has excellent comprehensive performance.
[0066] At 25°C, the tensile strength, yield strength and cross-sectional shrinkage of the quenched and tempered wire rod are tested in accordance with GB / T 228.1-2021; The notched specimens were processed according to GB / T 39039-2020. The specimens were electrochemically charged with hydrogen in 1000 mL of 4 g / L NaOH solution for 48 h at a current density of 15 A / m 2 After the hydrogen-filled samples were cleaned and dried, they were subjected to a 25°C tensile test on a slow strain rate tensile testing machine with a tensile strain rate of 5×10 -6 / s, and measure the tensile strength of the hydrogen-filled notch sample; the same parameters are used to test the non-hydrogen-filled notch sample to obtain the tensile strength of the non-hydrogen-filled notch sample; the delayed fracture strength ratio is calculated, and the delayed fracture strength ratio is the ratio of the tensile strength of the hydrogen-filled notch sample to the tensile strength of the non-hydrogen-filled notch sample; The specific results are shown in Table 5.
[0067] Table 5 Tensile strength / MPa Yield strength / MPa Sectional shrinkage / % Delayed rupture strength ratio Example 1 1289 1182 41 0.85 Example 2 1265 1164 42.3 0.84 Example 3 1278 1173 42.1 0.85 Example 4 1324 1215 40.2 0.83 Example 5 1267 1170 40.4 0.86 Example 6 1271 1172 41.8 0.85 Example 7 1264 1163 42.6 0.86 Example 8 1292 1189 41.5 0.84 Example 9 1343 1242 40.7 0.82 Example 10 1280 1175 41.8 0.83 Comparative Example 1 1127 1020 42.3 0.84 Comparative Example 2 1118 1029 42.6 0.85 Comparative Example 3 1271 1158 35.5 0.76 Comparative Example 4 1379 1268 34.2 0.75 Comparative Example 5 1136 1035 42.7 0.86 Comparative Example 6 1325 1196 33.5 0.73 Comparative Example 7 1179 1074 42.2 0.84 Comparative Example 8 1238 1131 36.4 0.75 Comparative Example 9 1183 1080 39 0.82 Comparative Example 10 1262 1165 37.7 0.79 In the present invention, when the tensile strength is ≥1220 MPa, it means that the strength of the prepared fastener is ≥12.9 grade. The data in the embodiment show that the wire rod prepared by the present invention can be used in 12.9 grade fastener steel after quenching and tempering.
[0068] In the present invention, the larger the delayed fracture strength ratio is, the better the delayed fracture resistance is. It is generally believed that a delayed fracture strength ratio of 0.8 or more is judged to be excellent, and the embodiments of the present invention all meet this data.
[0069] The wire rod of the embodiment of the present invention not only has good tensile properties and high strength after quenching and tempering, but also has excellent delayed fracture performance while meeting the strength requirements of 12.9-level fasteners. Among the comparative wire rods, the tensile properties of the wire rods of comparative examples 1, 2, 5, 7, and 9 after quenching and tempering do not meet the strength requirements of 12.9-level fasteners, and the delayed fracture performance of the wire rods of comparative examples 3, 4, 6, 8, and 10 after quenching and tempering is poor.
[0070] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.
Claims
1. A cold heading steel wire rod, characterized in that: Based on the mass of the wire rod, C: 0.25-0.30wt%, Si: 0.15-0.30wt%, Mn: 0.35-0.60wt%, P≤0.020wt%, S≤0.015wt%, Cr: 0.70-1.00wt%, Ni: 0.21-0.30wt%, Cu≤0.10wt%, Al: 0.015-0.050wt%, N≤0.007wt%, B: 0.0018-0.0030wt%, Ti: 0.020-0.035wt%, Re: 0.01-0.10wt%, and the rest are Fe and unavoidable impurities; The cross section of the wire rod is circular, and the ratio of the sum of the carbon and chromium contents at the center of the circle to the sum of the carbon and chromium contents at the 1 / 2 radius is 1.1-1.2:
1.
2. The wire rod according to claim 1, characterized in that The diameter of the wire rod is 20-40 mm.
3. The wire rod according to claim 1 or 2, characterized in that: The content of the Cr element and the content of the Mn element satisfy the formula Cr / Mn=1.5-2.0:
1.
4. The wire rod according to any one of claims 1 to 3, characterized in that: The content of the Ni element, the content of the Ti element, and the content of the Al element satisfy the formula Ni / (Ti+Al)=3.5-5:
1.
5. The wire rod according to any one of claims 1 to 4, characterized in that: The content of the C element, the content of the Cr element, the content of the Mn element, the content of the Ni element, and the content of the B element satisfy the formula (35×C+13×Cr+10×Mn+3×Ni+8000×B)×100≥43.
6. A method for preparing a cold heading steel wire rod according to any one of claims 1 to 5, characterized in that: The preparation method comprises the following steps: The molten iron is smelted, refined, continuously cast and rolled to obtain wire rods; Among them, during continuous casting, the superheat of the molten steel in the tundish is 30-40°C, and the drawing speed for billet straightening is 2.5-2.7m / min.
7. The preparation method according to claim 6, characterized in that: The smelting is converter smelting.
8. The preparation method according to claim 6 or 7, characterized in that: The refining is LF refining.
9. The preparation method according to any one of claims 6 to 8, characterized in that: The steel rolling includes heating, high-speed wire rolling and controlled cooling.
10. Use of the wire rod according to any one of claims 1 to 5 or the wire rod prepared by any one of claims 6 to 9 after quenching and tempering in 12.9 grade fastener steel; Optionally, the tempering treatment is: tempering the wire rod after quenching.
Citation Information
Patent Citations
Cr-B system low-carbon high-strength cold forging steel wire rod and manufacturing method thereof
CN110453150A
High-weather-resistant cold heading steel for 10.9 grade fastener and production method of high-weather-resistant cold heading steel
CN110923546A
Cold heading steel wire rod for annealing-free 10.9-grade fastener and manufacturing method of cold heading steel wire rod
CN113073259A
High-toughness cold heading and cold extruding steel 10B28 wire rod with nominal diameter of 16-20 mm and preparation method of high-toughness cold heading and cold extruding steel 10B28 wire rod
CN115305408A
Sulfur-added cold heading steel wire rod as well as preparation method and application thereof
CN116497261A