Stainless steel pipe for conveying high-purity gas and preparation method of stainless steel pipe
By using the composition of iron, chromium, nickel and other elements and multi-step process processing in the production of stainless steel pipes, a dense protective film and composite anti-corrosion layer are formed, which solves the problem of insufficient treatment of the inner wall roughness and welding interface of stainless steel pipes in the prior art. , realizes high-purity gas transportation and long-life equipment.
Patent Information
- Application Number
- CN202410999264.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing stainless steel pipe production process for high-purity gas delivery is difficult to achieve high cleanliness and corrosion resistance requirements, especially in terms of pipe inner wall surface roughness and welding interface treatment, which affects fluid transmission efficiency and equipment life.
Stainless steel pipes composed of iron, chromium, nickel and other elements are coiled and welded after solid solution and aging treatment, combined with cold rolling, annealing, pickling, water washing, electrochemical polishing and mechanical polishing to form a dense protective film , reduce the oxidation rate, and coat the inner surface with a composite anti-corrosion layer of epoxy resin and polyurethane to improve corrosion resistance and mechanical strength.
The prepared stainless steel pipe has better mechanical properties and corrosion resistance, reduced surface roughness of the inner wall, optimized fluid transmission efficiency, reduced equipment maintenance costs, and extended service life.
Smart Images

Figure BDA0004961105320000091 
Figure BDA0004961105320000101 
Figure BDA0004961105320000141
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of stainless steel parts preparation, and in particular to a stainless steel pipe for high-purity gas transportation and a preparation method thereof. Background Art
[0002] Stainless steel, also known as "acid-resistant stainless steel", is widely used in aerospace, marine, nuclear energy, medical equipment and petrochemical fields for its main characteristics of stainless steel, corrosion resistance and excellent mechanical properties. It is mainly used as fluid delivery pipelines for high-end products. Nowadays, with the continuous expansion of industrial scale and the continuous development of process technology, people's demand for stainless steel products is increasing, and the requirements for their use are getting higher and higher. In particular, the surface roughness of the inner wall of stainless steel pipes for transportation must reach Ra≤0.10μm or even lower, so as to reduce the resistance of the inner wall to the fluid and the adsorption of materials on the inner wall. However, the existing technology still cannot meet the high cleanliness requirements for the production process of stainless steel pipes for high-purity gas transportation. Therefore, it is urgent to study a stainless steel pipe for high-purity gas transportation and its preparation method. Summary of the invention
[0003] In order to solve at least one of the above technical problems, a stainless steel pipe with high surface finish and strong corrosion resistance is developed. The present application provides a stainless steel pipe for high-purity gas transportation and a preparation method thereof.
[0004] On the one hand, the present application provides a high-purity stainless steel pipe for gas transportation, which includes the following raw materials by mass: 70 to 80 parts of iron, 0.01 to 0.03 parts of carbon, 9 to 14 parts of nickel, 17 to 19 parts of chromium, 0.25 to 0.50 parts of silicon, 1.00 to 1.75 parts of manganese, 0.03 to 0.04 parts of phosphorus, 0.2 to 0.3 parts of sulfur, 2 to 3 parts of molybdenum and 0.2 to 0.6 parts of titanium.
[0005] By adopting the above technical scheme, elements such as iron, chromium, nickel, and manganese are used in the raw materials, so that a dense protective film can be formed on the surface of the stainless steel pipe, reducing its oxidation rate, so that the stainless steel pipe prepared in this application not only has better mechanical properties, but also has better corrosion resistance and a longer service life.
[0006] Optionally, the inner surface of the stainless steel pipe contains an anti-corrosion layer, and the anti-corrosion coating of the anti-corrosion layer is selected from epoxy resin coating and / or polyurethane coating.
[0007] Furthermore, the epoxy resin coating is a solvent-free epoxy resin coating and / or epoxy resin powder, and the polyurethane coating is a two-component polyurethane coating.
[0008] By adopting the above technical scheme, the epoxy resin coating has excellent bonding and anti-corrosion properties, and can form a balanced polymer network structure after curing, thereby giving the stainless steel pipe better rust resistance; polyurethane has good elasticity and flexibility, and can be used in application scenarios that require vibration resistance, impact resistance, etc.
[0009] Optionally, the anti-corrosion layer is a composite anti-corrosion layer, and the molar ratio of the epoxy resin coating to the polyurethane coating is (3-5):2.
[0010] By adopting the above technical solutions, the composite anti-corrosion coating can effectively isolate the direct contact between the steel pipe and the external environment, and can reduce the corrosion risk of the steel pipe regardless of acidic or alkaline conditions. The combination of the two can not only improve the mechanical strength and wear resistance of the stainless steel pipe as a whole, so that it can maintain its integrity for a long time, but also optimize the fluid transmission efficiency in the pipeline, protect the environment and save energy, thereby effectively reducing equipment maintenance costs and extending the service life of the equipment.
[0011] On the other hand, the present application provides a method for preparing the above-mentioned stainless steel pipe, comprising the following steps:
[0012] Step 1: Preparation of stainless steel plate: The raw materials are subjected to solid solution and aging treatment according to their mass fractions to obtain a stainless steel plate;
[0013] Step 2: Roll and weld the stainless steel plate processed in step 1 to obtain a stainless steel pipe;
[0014] Step 3: cold rolling and cleaning the stainless steel tube obtained in step 2, and then annealing;
[0015] Step 4: The stainless steel pipe after annealing in step 3 is pickled, washed and degreased in sequence;
[0016] Step 5, electrochemically polishing the stainless steel tube treated in step 4;
[0017] Step 6: The stainless steel tube treated in step 5 is subjected to passivation treatment, pure water rinsing treatment, and then drying;
[0018] Step 7, sandblasting and heating the inner surface of the stainless steel pipe treated in step 6, then coating the inner surface of the stainless steel pipe with an anti-corrosion layer, and finally cooling the stainless steel pipe to room temperature;
[0019] Step 8, mechanically polishing the inner surface of the stainless steel tube treated in step 7, and then rinsing with pure water;
[0020] Step nine, subjecting the stainless steel tube treated in step seven to hot nitrogen drying to obtain the stainless steel tube for high-purity gas transportation.
[0021] By adopting the above technical scheme, firstly, the cold-rolled and cleaned stainless steel pipe is annealed, which can not only avoid the formation of local high temperature during the annealing heating process, which affects the internal quality unevenness of the steel pipe material and the formation of surface quality defects, but also obtain stainless steel materials with better mechanical properties and antioxidant properties; secondly, after annealing, pickling, water washing and degreasing of the stainless steel material can effectively remove the oxide layer, welding slag and oxides generated during the heat treatment process on the surface of the stainless steel, thereby ensuring that the surface of the stainless steel material is completely clean and there is no substance that affects the passivation effect; finally, the stainless steel pipe is simultaneously subjected to electrochemical and mechanical polishing synergistic treatment, which can make the stainless steel pipe meet the requirements of high flatness and high gloss, and then obtain a lower inner wall surface roughness, so as to achieve the effect of reducing the inner wall's resistance to the fluid and the adsorption of materials on the inner wall, thereby ensuring the purity and quality of the product.
[0022] Optionally, the annealing treatment includes oxygen annealing treatment and oxygen-free bright annealing treatment in sequence.
[0023] By adopting the above technical scheme, aerobic annealing treatment initially improves the plasticity and toughness of the steel, and then the surface quality and oxidation resistance of the steel are improved by anaerobic bright annealing treatment, so that high-quality stainless steel materials can be obtained.
[0024] Optionally, in step five, the electrochemical polishing treatment includes: placing the stainless steel plate treated in step four in a chemical polishing solution at 75 to 80° C. for 8 to 12 minutes, then immersing the stainless steel tube in clean water at room temperature for 30 to 45 minutes, and finally rinsing with pure water.
[0025] Optionally, the chemical polishing solution contains 550-620 ml of phosphoric acid, 300-400 ml of nitric acid, 5.5-9.0 g of gelatin and 5.0-8.5 g of polyvinyl pyrrolidone per liter, and the balance is water.
[0026] By adopting the above technical scheme, phosphoric acid is the main luminescent muscle in the chemical polishing solution, which can significantly improve the brightness of the polished surface; nitric acid is directly related to the polishing effect of stainless steel materials, and an appropriate amount of nitric acid can help increase the brightness of steel. Excessive nitric acid will increase the corrosion rate of the polishing liquid on the workpiece, and also reduce the brightness of the polished surface, resulting in quality problems such as rough surface; gelatin can play a good corrosion inhibition role in the polishing process. It can react with phosphoric acid to form complexes and their metal derivatives. These complexes help to form a protective mucous membrane layer, thereby improving the quality and effect of steel polishing; polyvinyl pyrrolidone is a non-ionic polymer compound. Due to its excellent solubility and film-forming properties, it can not only improve the efficiency and quality of polishing in stainless steel electrochemical polishing, but also has certain economic benefits.
[0027] Optionally, in step seven, the inner surface of the stainless steel pipe treated in step six is sandblasted and heated, and then an anti-corrosion layer is coated on the inner surface of the stainless steel pipe, and finally the stainless steel pipe is cooled to room temperature, which specifically includes:
[0028] The inner surface of the stainless steel pipe after the treatment in step six is sequentially sandblasted and dusted, and then the stainless steel pipe is subjected to medium frequency heating, and then the anti-corrosion coating is applied to the inner surface of the stainless steel pipe by electrostatic spraying, and finally cooled by pure water.
[0029] By adopting the above technical solution, the anti-corrosion layer can be evenly adsorbed on the inner wall of the steel pipe, thereby further enhancing the corrosion resistance of the steel.
[0030] Optionally, during the electrostatic spraying treatment, the temperature of the surface of the stainless steel plate is 200-230°C.
[0031] By adopting the above technical solution, the anti-corrosion layer can be fully coated and the coating can have a certain glossiness.
[0032] Optionally, in step eight, the mechanical polishing treatment includes: rough polishing, semi-fine polishing and fine polishing treatment in sequence; wherein, during the rough polishing, the rotation speed of the polishing machine is 35000-40000 r / min; and the semi-fine polishing uses 320-400 mesh sandpaper.
[0033] By adopting the above technical solution, the high-speed rough polishing method can not only remove the defects and unevenness on the material surface, but also effectively improve the polishing efficiency of the subsequent fine polishing; higher-grit sandpaper polishing can further improve the cleanliness of the steel surface; and the use of abrasive paste in the final fine polishing can achieve the best polishing effect.
[0034] In summary, the present invention includes at least one of the following beneficial technical effects:
[0035] 1. The stainless steel pipe produced by the present application not only has better mechanical properties, but also has better corrosion resistance and longer service life.
[0036] 2. The method for preparing a stainless steel pipe for high-purity gas in the present application, first, cold-rolling and cleaning the stainless steel pipe and then annealing it, can not only avoid the formation of local high temperature during the annealing heating process, which affects the internal quality unevenness of the steel pipe material and the formation of surface quality defects, but also obtain stainless steel materials with better mechanical properties and antioxidant properties; secondly, after annealing, pickling, water washing and degreasing the stainless steel material can effectively remove the oxide layer, welding slag and oxides generated during the heat treatment process on the surface of the stainless steel, thereby ensuring that the surface of the stainless steel material is completely clean and there is no substance that affects the passivation effect; finally, electrochemical and mechanical polishing are synergistically treated on the stainless steel pipe, so that the inner wall surface of the stainless steel pipe can meet the requirements of high flatness and high gloss, thereby obtaining a lower inner wall surface roughness, so as to achieve the effect of reducing the inner wall's resistance to the fluid and reducing the adsorption of materials on the inner wall, thereby ensuring the purity and quality of the product. DETAILED DESCRIPTION
[0037] The present application is further described in detail below with reference to the embodiments.
[0038] The present application designs a stainless steel pipe for high-purity gas, which includes the following raw materials by mass: 70-80 parts of iron, 0.01-0.03 parts of carbon, 9-14 parts of nickel, 17-19 parts of chromium, 0.25-0.50 parts of silicon, 1.00-1.75 parts of manganese, 0.03-0.04 parts of phosphorus, 0.2-0.3 parts of sulfur, 2-3 parts of molybdenum and 0.2-0.6 parts of titanium.
[0039] When designing the above-mentioned stainless steel pipe, the present application also coats the pipe wall with an anti-corrosion coating, and the anti-corrosion coating of the anti-corrosion layer is selected from epoxy resin coating and / or polyurethane coating.
[0040] On the basis of the above, the applicant further determined that the anti-corrosion layer is a composite anti-corrosion layer, and limited the molar ratio of the epoxy resin coating to the polyurethane coating to (3-5):2.
[0041] The present application also provides a method for preparing the above-mentioned high-purity gas stainless steel pipe, comprising the following steps:
[0042] Step 1: Preparation of stainless steel plate: The raw materials are subjected to solid solution and aging treatment according to their mass fractions to obtain a stainless steel plate;
[0043] Step 2: Roll and weld the stainless steel plate processed in step 1 to obtain a stainless steel pipe;
[0044] Step 3: cold rolling and cleaning the stainless steel tube obtained in step 2, and then annealing;
[0045] Step 4: The stainless steel pipe after annealing in step 3 is pickled, washed and degreased in sequence;
[0046] Step 5, electrochemically polishing the stainless steel tube treated in step 4;
[0047] Step 6: The stainless steel tube treated in step 5 is subjected to passivation treatment, pure water rinsing treatment, and then drying;
[0048] Step 7, sandblasting and heating the inner surface of the stainless steel pipe treated in step 6, then coating the inner surface of the stainless steel pipe with an anti-corrosion layer, and finally cooling the stainless steel pipe to room temperature;
[0049] Step 8, mechanically polishing the inner surface of the stainless steel tube treated in step 7, and then rinsing with pure water;
[0050] Step nine, subjecting the stainless steel tube treated in step seven to hot nitrogen drying to obtain the stainless steel tube for high-purity gas transportation.
[0051] On the basis of the above, the applicant further optimized the preparation steps, the annealing treatment includes aerobic annealing treatment and oxygen-free bright annealing treatment, and the polishing treatment includes electrochemical polishing treatment and mechanical polishing treatment.
[0052] With the rapid development of science and technology, the application of high-purity gas is becoming more and more extensive, and the requirements for stainless steel pipes used for its transportation are becoming increasingly stringent, especially the problem of the cleanliness of the inner surface of the pipe. However, the main factors affecting the cleanliness of the inner surface of the pipe include: polishing technology, problems in the annealing process, and the treatment of the welding joint.
[0053] Prior to the present invention, the use of existing high-purity gas stainless steel pipes usually focuses on the improvement of polishing technology when improving the finish / cleanliness of the inner wall of the pipe. By continuously improving and updating the components of the electrochemical polishing liquid, the corrosion degree of the steel is reduced, thereby ensuring the polishing quality, thereby obtaining a relatively excellent surface cleanliness of the inner wall of the stainless steel pipe. However, the electrolytic polishing effect is limited, and due to the particularity of the pipe structure, the inner surface of the steel pipe is difficult to clean after electrolytic polishing, resulting in impurities and other residues that affect the quality and transmission efficiency of the gas, and still cannot meet the requirements of high-purity gas delivery. In addition, the problems in the annealing process and the treatment of the weld joints have not been properly solved.
[0054] In order to fully consider and solve the above technical problems as much as possible, the inventors made the present invention through further research.
[0055] First, when considering the problems that arise during the annealing process, the inventor chose to anneal the stainless steel pipe after cold rolling and cleaning, and the annealing method was a combination of aerobic annealing and anaerobic bright annealing. During the annealing process, if only aerobic annealing is used, although it can effectively improve the plasticity and toughness of the steel, in the production process of stainless steel pipes, aerobic annealing will cause the surface of the steel pipe to be oxidized by oxygen in the air, generating an iron oxide surface, thereby reducing the surface finish of the inner tube, and sometimes forming defects such as bulges on the inner surface of the tube; and anaerobic bright annealing is easily affected by factors such as processing temperature, marks, and atmosphere. If the bright annealing temperature is set too high, the surface finish of the stainless steel water pipe will deteriorate, and the ability of the stainless steel surface to bond to the treatment liquid will also be reduced, that is, poor brightness will be caused; in addition, if a deeper mark is left during the processing of the stainless steel water pipe, it will also cause poor brightness in that part; if the gas type and atmosphere are not well adapted during vacuum bright annealing, it will also cause problems such as uneven light and defects. Therefore, the cold-rolled cleaned stainless steel pipe is annealed after treatment, and a combination of aerobic annealing and anaerobic bright annealing is selected. This can not only avoid the formation of local high temperature during the annealing heating process, which affects the uneven internal quality of the steel pipe material and the formation of surface quality defects, but also obtain stainless steel materials with better mechanical properties and antioxidant properties.
[0056] Secondly, when solving the polishing problem, the inventors took into account the treatment of the welding machine mouth and adopted a strategy of combined electrochemical polishing and mechanical polishing in the process of preparing stainless steel pipes. This can make the stainless steel pipes meet the requirements of high flatness and high gloss, and thus obtain a lower inner wall surface roughness, so as to achieve the effect of reducing the inner wall's resistance to the fluid and reducing the adsorption of materials on the inner wall, thereby ensuring the purity and quality of the product.
[0057] The present application is further described below in conjunction with specific examples. Unless otherwise specified, the materials used in the preparation examples and examples are all commercially available conventional materials.
[0058] Table 1 shows the composition of the stainless steel plates of Preparation Examples 1 to 10.
[0059]
[0060] Preparation Examples 1 to 10 are prepared according to conventional methods, such as preparing stainless steel plates, including: melting the constituent raw materials of each preparation example at high temperature, injecting the molten liquid into a mold to form a steel billet, subjecting the steel billet to a pressing and rolling process, cutting it to a desired shape and size, and then heat treating and cooling it.
[0061] The stainless steel plates obtained in Preparation Examples 1 to 10 were subjected to appearance inspection, mechanical property test and corrosion resistance test, and the test results are recorded in Table 2 below.
[0062] (1) Appearance inspection
[0063] By visually inspecting the surface of the stainless steel plate to see if it is smooth and has no defects, we can preliminarily judge whether its quality is qualified;
[0064] (2) Mechanical properties test
[0065] According to the relevant records in the national standard GB / T20878-2007, the tensile strength, yield strength and elongation are tested accordingly;
[0066] (3) Corrosion resistance test
[0067] The stainless steel tubes prepared in Preparation Examples 1 to 10 were placed in a sulfuric acid solution with a mass fraction of 60%, and corroded at room temperature for 72 hours to detect the corrosion degree of the sulfuric acid solution on the stainless steel tubes.
[0068] Table 2 Performance test results of stainless steel plates of Preparation Examples 1 to 10
[0069]
[0070] From the performance test results in Table 2, it can be seen that the stainless steel plates prepared in this application have good mechanical properties and good corrosion resistance. In addition, combined with the composition raw material data in Table 1, we can also find that chromium plays a key role in the corrosion resistance of stainless steel plates, and the addition of nickel and molybdenum can further improve the corrosion resistance and corrosion resistance of stainless steel plates.
[0071] The following are Examples 1 to 6 of the present invention. The stainless steel pipes prepared in Examples 1 to 6 are based on the stainless steel plates prepared in Preparation Examples 1 to 6 as reference materials. The stainless steel pipe for high-purity gas transportation is obtained by the preparation method of the stainless steel pipe of the present invention.
[0072] Taking Example 1 as an example, the preparation steps specifically include the following:
[0073] Step 1, refer to the production method of the preparation example;
[0074] Step 2: Roll and weld the stainless steel plate processed in step 1 to obtain a stainless steel tube a;
[0075] Step 3: cold rolling and cleaning the stainless steel tube a obtained in step 2, and then performing an aerobic annealing treatment to obtain a stainless steel tube b; cold rolling and cleaning the stainless steel tube b for a second time, and performing an oxygen-free bright annealing treatment to obtain a stainless steel tube c;
[0076] Step 4: The stainless steel tube c in step 3 is sequentially subjected to pickling treatment, water washing treatment, and degreasing treatment to obtain a stainless steel tube d;
[0077] Step 5, electrochemically polishing the stainless steel tube d in step 4, including preparing a chemical polishing solution containing 580 ml of phosphoric acid, 320 ml of nitric acid, 6.4 g of gelatin and 6.0 g of polyvinyl pyrrolidone per liter, and the balance being water, placing the stainless steel tube d in the chemical polishing solution at 80° C. for 10 minutes, then immersing it in clean water at room temperature for 35 minutes, and finally rinsing the steel tube with pure water to obtain a stainless steel tube e;
[0078] Step 6: The stainless steel tube e in step 5 is subjected to passivation treatment and pure water rinsing treatment in sequence, and then dried by hot nitrogen blowing to obtain a stainless steel tube f;
[0079] Step 7, after spraying quartz sand on the inner surface of the stainless steel pipe f in step 6, the anti-corrosion composite coating is applied to the inner surface of the stainless steel pipe by medium frequency heating, and the molar ratio of the epoxy resin material to the polyurethane coating is 3:2. The temperature of the steel pipe is kept at 210° C. during electrostatic spraying, and finally the steel pipe is cooled to room temperature to obtain a stainless steel pipe g;
[0080] Step 8, the inner surface of the stainless steel tube g in step 7 is subjected to rough polishing, semi-fine polishing and fine polishing in sequence. First, the polishing machine is used for rough polishing at a speed of 35000 r / min; secondly, the inner wall of the steel tube is polished with 400-mesh sandpaper, and finally, the grinding paste is used for fine polishing, and then the steel tube is rinsed with pure water to obtain the stainless steel tube h;
[0081] Step 9: In a clean room, the stainless steel tube h in step 7 is dried with hot nitrogen to obtain the stainless steel tube for high-purity gas delivery.
[0082] The stainless steel pipes of Examples 2 to 6 can be prepared by referring to the steps of Example 1 without departing from the protection scope of the present application.
[0083] Comparative Example 1
[0084] The difference from Example 1 is that in step 3, annealing is directly performed without cold rolling and cleaning.
[0085] Comparative Example 2
[0086] The difference from Example 2 is that in step 3, no cold rolling and cleaning is performed, and only oxygen-free bright annealing is performed.
[0087] Comparative Example 3
[0088] The difference from Example 3 is that step seven and step eight are omitted.
[0089] The inventors tested the corrosion resistance and surface roughness of the stainless steel pipes prepared in the above-mentioned Examples 1 to 6 and Comparative Examples 1 to 3, and recorded the test results in the following Table 3. Among them, the corrosion resistance is to take the stainless steel pipes prepared in Examples 1 to 6 and Comparative Examples 1 to 3, place them in a sulfuric acid solution with a mass fraction of 60%, and corrode them at room temperature for 72 hours to detect the corrosion degree of the sulfuric acid solution on the stainless steel pipe; the surface roughness is measured by using the Japanese Mitutoyo SJ-210 roughness meter to detect the surface roughness of the two ends (the average of the upper and lower corresponding points) and the center (the average of the upper and lower corresponding points) of the steel pipe, and record them as Ra1, Ra2, and Ra3 ends respectively.
[0090] Table 3 Performance test results of stainless steel pipes of Examples 1 to 6 and Comparative Examples 1 to 3
[0091] Corrosion rate mm / year <![CDATA[Ra1 / μm]]> <![CDATA[Ra2 / μm]]> <![CDATA[Ra3 / μm]]> Example 1 0.0027 0.023 0.021 0.022 Example 2 0.0018 0.016 0.018 0.012 Example 3 0.0020 0.015 0.015 0.014 Example 4 0.0023 0.020 0.018 0.015 Example 5 0.0009 0.008 0.008 0.006 Example 6 0.0010 0.008 0.007 0.006 Comparative Example 1 0.0048 0.074 0.076 0.074 Comparative Example 2 0.0057 0.088 0.085 0.085 Comparative Example 3 0.0045 0.082 0.089 0.089
[0092] It can be seen from the performance test results in Table 3 that the preparation method of the stainless steel pipe of the present application can not only effectively slow down the corrosion rate of the inner wall of the pipe, but also has a low surface roughness, thereby ensuring the purity and quality of the product. In addition, in combination with the performance test data results of Example 1 and Comparative Example 1, Example 2 and Comparative Example 2, and Example 3 and Comparative Example 3, we can find that: the annealing treatment after cold rolling and cleaning the stainless steel pipe can fully avoid the formation of local high temperature during the annealing and heating process, which affects the inherent quality unevenness of the steel pipe material and the formation of surface quality defects. The electrochemical and mechanical polishing synergistic treatment of the stainless steel pipe can make the stainless steel pipe meet the requirements of high flatness and high gloss, thereby obtaining a lower inner wall surface roughness, so as to achieve the effect of reducing the inner wall resistance to the fluid and the adsorption of the material on the inner wall, thereby ensuring the purity and quality of the product as a whole.
[0093] The inventors found through practice that the ratio of epoxy resin coating to polyurethane coating in the anti-corrosion composite layer will further affect the anti-corrosion performance of the inner wall of the stainless steel pipe, and the inner wall of the stainless steel pipe will also have a certain impact on the purity and quality of the transported gas due to corrosion. Taking Example 1 as an example, the inventors prepared Examples 7 to 9 by adjusting the ratio of epoxy resin coating to polyurethane coating. The stainless steel pipes prepared in Examples 7 to 9 were respectively tested for corrosion at room temperature for 72 hours in 60wt% sulfuric acid solution and sodium hydroxide solution, and the corrosion degree of the sulfuric acid solution and sodium hydroxide solution on the stainless steel pipe was detected, and the test results were recorded in Table 4 below.
[0094] Table 4 Corrosion test results of Example 1 and Examples 7 to 9 in acid and alkali solutions
[0095]
[0096] It can be seen from the test results in Table 4 that in the present application, when the molar ratio of the epoxy resin coating to the polyurethane coating is controlled between 3: (2-5), the stainless steel pipe exhibits excellent corrosion resistance in both acidic and alkaline environments; and when the molar ratios of the two coatings differ greatly, the stainless steel pipe will exhibit greatly different corrosion resistance under different conditions, and the fluctuations affected by environmental factors are obvious, which is not convenient for industrial variable operations.
[0097] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. A stainless steel pipe for high-purity gas transportation, characterized in that: The stainless steel pipe includes the following raw materials by mass: 70-80 parts of iron, 0.01-0.03 parts of carbon, 9-14 parts of nickel, 17-19 parts of chromium, 0.25-0.50 parts of silicon, 1.00-1.75 parts of manganese, 0.03-0.04 parts of phosphorus, 0.2-0.3 parts of sulfur, 2-3 parts of molybdenum and 0.2-0.6 parts of titanium.
2. The stainless steel pipe for high-purity gas transportation according to claim 1, characterized in that: The inner surface of the stainless steel pipe comprises an anti-corrosion layer, and the anti-corrosion coating of the anti-corrosion layer is selected from epoxy resin coating and / or polyurethane coating; Preferably, the epoxy resin coating is a solvent-free epoxy resin coating and / or epoxy resin powder, and the polyurethane coating is a two-component polyurethane coating.
3. The stainless steel pipe for high-purity gas transportation according to claim 2, characterized in that: The anti-corrosion layer is a composite anti-corrosion layer, and the molar ratio of the epoxy resin coating to the polyurethane coating is (3-5):
2.
4. A method for preparing a high-purity stainless steel pipe for gas transportation as claimed in any one of claims 1 to 3, characterized in that: The following steps are involved: Step 1: Preparation of stainless steel plate: The raw materials are subjected to solid solution and aging treatment according to their mass fractions to obtain a stainless steel plate; Step 2: Roll and weld the stainless steel plate processed in step 1 to obtain a stainless steel pipe; Step 3: cold rolling and cleaning the stainless steel tube obtained in step 2, and then annealing; Step 4: The stainless steel pipe after annealing in step 3 is pickled, washed and degreased in sequence; Step 5, electrochemically polishing the stainless steel tube treated in step 4; Step 6: The stainless steel tube treated in step 5 is subjected to passivation treatment, pure water rinsing treatment, and then drying; Step 7, sandblasting and heating the inner surface of the stainless steel pipe treated in step 6, then coating the inner surface of the stainless steel pipe with an anti-corrosion layer, and finally cooling the stainless steel pipe to room temperature; Step 8, mechanically polishing the inner surface of the stainless steel tube treated in step 7, and then rinsing with pure water; Step nine, subjecting the stainless steel tube treated in step seven to hot nitrogen drying to obtain the stainless steel tube for high-purity gas transportation.
5. The preparation method according to claim 4, characterized in that: In step three, the annealing treatment includes oxygen annealing treatment and oxygen-free bright annealing treatment in sequence.
6. The preparation method according to claim 4, characterized in that: In step 5, the electrochemical polishing treatment includes: placing the stainless steel plate treated in step 4 in a chemical polishing solution at 75 to 80° C. for 8 to 12 minutes, then immersing the stainless steel tube in clean water at room temperature for 30 to 45 minutes, and finally rinsing with pure water.
7. The preparation method according to claim 6, characterized in that: The chemical polishing solution contains 550-620 ml of phosphoric acid, 300-400 ml of nitric acid, 5.5-9.0 g of gelatin and 5.0-8.5 g of polyvinyl pyrrolidone per liter, and the balance is water.
8. The preparation method according to claim 4, characterized in that: In step seven, the inner surface of the stainless steel pipe treated in step six is sandblasted and heated, and then an anti-corrosion layer is coated on the inner surface of the stainless steel pipe, and finally the stainless steel pipe is cooled to room temperature, which specifically includes: The inner surface of the stainless steel pipe after the treatment in step six is sequentially subjected to sandblasting and surface dust removal treatments, and then the stainless steel pipe is subjected to medium frequency heating, and then an anti-corrosion coating is applied to the inner surface of the stainless steel pipe by electrostatic spraying, and finally cooled by pure water.
9. The preparation method according to claim 8, characterized in that: During the electrostatic spraying treatment, the surface temperature of the stainless steel plate is 200-230°C.
10. The preparation method according to claim 4, characterized in that: In step eight, the mechanical polishing treatment includes: rough polishing, semi-finishing polishing and fine polishing treatment in sequence; wherein, during the rough polishing, the rotation speed of the polishing machine is 35000-40000 r / min; and the semi-finishing polishing uses 320-400 mesh sandpaper.
Citation Information
Cited By
Production equipment and processing method of clean pipe for semiconductor
CN119458121A