Alloy wear-resistant material for adjusting wear resistance based on WC content and preparation method of alloy wear-resistant material
By adjusting the WC addition amount in the iron-based shape memory alloy, alloy wear-resistant materials are prepared, which solves the problem that alloy materials are difficult to take into account both wear resistance and deformation recovery rate, broadens its application range in the industrial field, and improves the material hardness and wear resistance.
Patent Information
- Application Number
- CN202411112563.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing alloy materials are difficult to take into account both wear resistance and deformation recovery, which limits their application range in the industrial field.
By adjusting the amount of WC addition in the iron-based shape memory alloy, the alloy wear-resistant material is prepared by laser fuse deposition additives, and the content of WC is adjusted to change the material's wear resistance and other properties such as hardness and shape recovery.
The possibility of wider application of alloy materials in the industrial field is realized. By adjusting the WC content and selecting the appropriate material properties according to actual needs, the hardness and wear resistance of the material are improved while taking into account the shape recovery rate.
Smart Images

Figure CN118932257A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of alloy strengthening, in particular to an alloy wear-resistant material with wear resistance adjusted based on WC content and a preparation method thereof. Background Art
[0002] Wear resistance, hardness, deformation recovery rate, etc. are all evaluation attributes of alloy performance. Generally speaking, the stronger the wear resistance of the alloy, the higher its hardness, resulting in a worse deformation recovery rate. When common alloy materials are used to manufacture precision parts, it is impossible to take into account both wear resistance and deformation recovery rate. Of course, there are exceptions, such as iron-based shape memory alloys, which have unique anti-friction and anti-wear properties, and have certain advantages in processing complex-shaped metal parts with shape memory functions, but due to their relatively low hardness, their processing and forming properties are poor, and it is difficult to use traditional processes to form complex precision parts, which also limits their application in the industrial field. Summary of the invention
[0003] Purpose of the invention: In order to overcome the deficiencies in the prior art, the present invention provides an alloy wear-resistant material whose wear resistance is adjusted based on the WC content and a preparation method thereof, so as to solve the problem that the alloy material performance lacks more choices in maintaining a relatively balanced combination of multiple properties such as wear resistance, hardness, and deformation recovery rate, and broaden the application scope of the alloy material in the industrial field.
[0004] Technical solution: To achieve the above-mentioned purpose, the alloy wear-resistant material with wear resistance adjusted based on WC content and its preparation method are prepared by laser fuse deposition additive manufacturing and are marked as matrix-xWC alloy wear-resistant material, wherein the material matrix is an iron-based shape memory alloy, x is the value of the WC addition amount in the alloy wear-resistant material, x∈[0.25,4]; when the WC addition amount is 0.25-1wt.%, the wear resistance of the alloy wear-resistant material is on a downward trend; when the WC addition amount is 1-4wt.%, the wear resistance of the alloy wear-resistant material is on an upward trend.
[0005] Furthermore, the material matrix is Fe-Mn-Si-Cr-Ni alloy, and the prepared alloy wear-resistant material is marked as Fe-Mn-Si-Cr-Ni-xWC alloy, x∈[0.25,4], among which the Fe-Mn-Si-Cr-Ni-0.25WC alloy wear-resistant material has the highest wear resistance.
[0006] Furthermore, when the WC addition amount is 0.25wt.%, there are no obvious WC particles in the alloy deposition morphology, and as the WC addition amount increases, the WC particle density increases.
[0007] Furthermore, when 0.25-1wt.% WC is added, the added WC decomposes, and the released tungsten element is partially dissolved in the material matrix, and the tungsten element exceeding the solid solubility limit reacts with iron and carbon elements to generate Fe6W6C type carbides.
[0008] Furthermore, when 0.25-1wt.% WC is added, as the WC content increases, in the sub-surface morphology of the alloy wear-resistant material after friction and wear, the number of martensite laths decreases and the spacing between martensite increases; wherein, the increase in WC content leads to an increase in the content of Fe6W6C, and the Fe6W6C carbide particles hinder the sliding of the slip band of the material matrix, thereby inhibiting the formation of martensite and hindering the positive phase transformation of part of the austenite to martensite, so as to weaken the unique friction reduction and wear resistance of the material matrix.
[0009] Further, when 1-4 wt. % WC is added, undissolved WC hard particles appear, and as the content of WC increases, the density of WC hard particles in the alloy wear-resistant material increases.
[0010] Furthermore, when 0.25-4 wt. % WC is added, the memory property of the alloy wear-resistant material gradually decreases as the content of WC increases.
[0011] Further, when 0.25-2wt.% WC is added, the hardness of the alloy wear-resistant material increases as the content of WC increases; and when 2-4wt.% WC is added, the hardness of the alloy wear-resistant material remains unchanged.
[0012] Further, the following steps are included:
[0013] Step I, preparing a powder core wire, wrapping a mixed alloy powder with an alloy tube as an outer skin, and drawing to form a wire material with uniform diameter; the main components of the powder core wire are Fe, Mn, Si, Cr, Ni and WC; wherein, the same material alloy outer skin a is used and mixed alloy powder b with different WC content is used to prepare powder core wires with various WC contents, and the WC content is within the range of 0.25-4wt.%;
[0014] Step II, using laser cladding technology, feeding the powder core wire to the alloy substrate at a uniform speed, and stacking layer by layer to form a thin-wall coating to form an alloy wear-resistant material; wherein the powder core wires with different WC contents are laser clad with the alloy substrate of the same material to form alloy wear-resistant materials with different WC contents;
[0015] Step III, sampling the alloy wear-resistant materials with different WC contents, and conducting friction and wear tests, wear scar subsurface morphology observation, deposited structure observation, alloy hardness test and shape recovery characteristic test respectively;
[0016] Step IV, by comparing the results of each experiment and observation with the expected characteristics of the target material, using the W content value in step I as the end value of the new value range to narrow the value range;
[0017] Step V, repeating the above steps I to IV, wherein the WC content in step I is taken within the narrowed value range until the WC addition amount corresponding to the expected target material is obtained;
[0018] Step VI: repeat the above steps I to II according to the obtained WC addition amount to prepare an alloy wear-resistant material with expected properties.
[0019] Furthermore, after the friction and wear experiment, the middle part of the wear scar was horizontally cut into samples for observation of the subsurface morphology of the wear scar; the samples for observation of the deposited structure and the subsurface morphology of the wear scar were prepared into metallographic samples, and after being etched by the corrosive liquid, the microstructure morphology was observed by electron microscope; the bending deformation method was adopted to determine the shape recovery characteristics of the alloy wear-resistant material. Under normal temperature conditions, the alloy sample was subjected to a predetermined deformation treatment using a bending mold. After standing for a period of time, the recovery angle θ of the sample after pressure unloading was measured. e and the recovery angle θ after standing for a period of time m , calculate the shape recovery rate η; calculate the pre-deformation ε of the sample by the sample thickness t and the mold diameter D; where:
[0020]
[0021] The shape recovery rate and the pre-deformation ε are used to evaluate the shape memory effect.
[0022] Beneficial effects: The alloy wear-resistant material with wear resistance adjusted based on WC content and the preparation method thereof of the present invention can change the wear resistance of the prepared alloy wear-resistant material by adjusting the amount of WC added, and there may be multiple other properties corresponding to the same wear resistance, such as hardness, shape recovery rate, etc., and then the appropriate amount of WC added can be selected according to the actual application requirements for material hardness, shape recovery rate and other properties, so that the prepared alloy material is more in line with the application requirements, greatly improving the application scope of this type of alloy material in the industrial field. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a schematic diagram of the cross-sectional structure of the powder core wire material of the present invention;
[0024] Figure 2 OM images of the deposited state of multiple embodiments of the Fe-Mn-Si-Cr-Ni-xWC alloy of the present invention;
[0025] Figure 3XRD diagrams of the deposited state of multiple embodiments of the Fe-Mn-Si-Cr-Ni-xWC alloy of the present invention;
[0026] Figure 4 The subsurface SEM images of multiple embodiments of the Fe-Mn-Si-Cr-Ni-xWC alloy of the present invention;
[0027] Figure 5 It is a recovery rate trend diagram of multiple embodiments of the Fe-Mn-Si-Cr-Ni-xWC alloy of the present invention under 4% pre-deformation;
[0028] Figure 6 Volume wear rate curves and hardness curves of multiple embodiments of the Fe-Mn-Si-Cr-Ni-xWC alloy of the present invention;
[0029] Figure 7 This is a schematic diagram of the state of measuring the shape recovery characteristics of alloy wear-resistant materials using the bending deformation method of the present invention. DETAILED DESCRIPTION
[0030] The present invention will be further described below in conjunction with the accompanying drawings.
[0031] As attached Figure 1-7 The alloy wear-resistant material and its preparation method for adjusting wear resistance based on WC content are prepared by laser fuse deposition additive manufacturing and are marked as matrix-xWC alloy wear-resistant material, wherein the material matrix is an iron-based shape memory alloy. Preferably, the material matrix is a Fe-Mn-Si-Cr-Ni alloy, and the prepared alloy wear-resistant material is marked as a Fe-Mn-Si-Cr-Ni-xWC alloy. The Fe-Mn-Si-Cr-Ni alloy is a type of corrosion-resistant iron-based shape memory alloy that induces austenite to martensite positive and negative phase transformation to achieve shape memory effect, and the induction of its austenite to martensite positive and negative phase transformation originates from the reversible movement of Shockley incomplete dislocations induced by stress. Fe-Mn-Si-Cr-Ni alloy has the advantages of low cost, high strength, phase transition temperature close to room temperature, good corrosion resistance, etc., and it also exhibits unique anti-friction and anti-wear properties during friction and wear. In terms of friction reduction, the contact stress during friction and wear will cause the Fe-Mn-Si-Cr-Ni shape memory alloy to produce stress-induced martensite, that is, part of the force acts as the driving force for the phase transformation of austenite to martensite, thereby reducing the contact stress acting on the alloy during friction. In terms of wear resistance, martensite has higher hardness and lower adhesion coefficient than austenite.
[0032] x is the value of the WC addition in the alloy wear-resistant material, x∈[0.25,4]; when the WC addition is 0.25wt.%, there are no obvious WC particles in the alloy deposition morphology, and as the WC addition increases, the WC particle density increases.
[0033] The wear mechanism of the alloy wear-resistant material in this scheme is divided into two stages. In the first stage, when 0.25-1wt.% WC is added, the wear is mainly dominated by the inherent friction reduction and wear resistance of the Fe-Mn-Si-Cr-Ni alloy; in the second stage, the WC addition amount is increased to 1-4wt.%, which is mainly dominated by the dispersion strengthening effect of WC particles. As a result, when the WC addition amount is 0.25-1wt.%, the wear resistance of the alloy wear-resistant material is on a downward trend; when the WC addition amount is 1-4wt.%, the wear resistance of the alloy wear-resistant material is on an upward trend. Among them, the Fe-Mn-Si-Cr-Ni-0.25WC alloy wear-resistant material has the highest wear resistance.
[0034] The principle is:
[0035] When 0.25-1wt.% WC is added, the added WC is completely decomposed during the heating process, and the released tungsten element is partially dissolved in the material matrix. The tungsten element exceeding the solid solubility limit reacts with iron and carbon elements to generate Fe6W6C type carbides. As the content of WC increases, in the subsurface morphology of the alloy wear-resistant material after friction and wear, the number of martensite laths decreases and the spacing of martensite increases; wherein, the increase in the content of WC leads to an increase in the content of Fe6W6C, and the Fe6W6C carbide particles hinder the sliding of the slip band of the material matrix, which is used to inhibit the formation of martensite and hinder the positive phase transformation of part of austenite to martensite, so as to weaken the unique anti-friction and anti-wear properties of the material matrix.
[0036] When 1-4wt.% WC is added, undissolved WC hard particles appear, and as the WC content increases, the density of WC hard particles in the alloy wear-resistant material increases.
[0037] In addition, when 0.25-4wt.% WC is added, the memory property of the alloy wear-resistant material gradually decreases as the content of WC increases. When 0.25-2wt.% WC is added, the hardness of the alloy wear-resistant material increases as the content of WC increases; when 2-4wt.% WC is added, the hardness of the alloy wear-resistant material remains unchanged.
[0038] The above is the law of performance changes of the alloy wear-resistant material prepared by this scheme under the influence of WC content. It can be seen that compared with the shape memory alloy without adding WC, the hardness has been significantly improved, which is enough to meet the hardness requirements of complex precision parts formed by traditional processes. With the increase of WC content, the hardness shows an upward trend, but the increase is small, and when it rises to a certain upper limit, the hardness will no longer increase, so that the hardness of the overall material can meet the molding requirements while not increasing indefinitely and increasing the difficulty of processing. In addition, with the increase of WC content, the change of wear resistance shows a broken line change trend, while the corresponding hardness and shape recovery rate change curve is a unidirectional change trend, so that the prepared alloy material with the same wear resistance may correspond to two or more hardness and shape recovery rate properties, so that according to the actual requirements for the performance of the alloy material, the performance can be adjusted and selected by adjusting the WC content. For example, with specific wear resistance as the main goal, the WC content corresponding to the wear resistance is obtained through repeated experiments. There may be multiple results for the WC content. At this time, the selection is made based on the requirements for hardness and shape recovery rate, and finally a more appropriate WC addition amount is determined to prepare the alloy wear-resistant material that best meets the requirements. And when the wear resistance of the alloy wear-resistant material is good, the shape recovery rate is also good, and the hardness is relatively low. It is more suitable for forming into high-wear-resistant precision parts with shape memory function through processing techniques such as stamping and bending. When the wear resistance is relatively low, the shape recovery rate is correspondingly low, and the hardness is relatively high, which is suitable for turning and milling and other processes. Processing into wear-resistant fixed-shape high-precision parts has significantly increased its application field.
[0039] The specific WC addition amount positioning and material preparation process include the following steps:
[0040] Step I, prepare powder core wire, adopt the round tube method, wrap the mixed alloy powder with alloy pipe as the outer skin, and use the customized size rolling and drawing integrated device to draw to form a wire material with uniform diameter; the main components of the powder core wire are Fe, Mn, Si, Cr, Ni and WC, and the proportion of each component is 1:17:6:9:5:x; wherein, the alloy pipe is preferably 304 stainless steel pipe, and its main components are Fe, Cr, Ni; the main components of the uniformly mixed alloy powder are Fe, Mn, Si, Cr, Ni and WC. It can inhibit the uneven burning of elements in the alloy, and it is easy to control the composition.
[0041] A plurality of powder core wires with different WC contents are prepared by using alloy sheath a of the same material and mixed alloy powder b with different WC contents, wherein the WC content is within the range of 0.25-4wt.%.
[0042] Step II, using laser cladding technology, the powder core wire is fed to the alloy substrate at a uniform speed, and is deposited layer by layer to form a thin-wall coating to form an alloy wear-resistant material; wherein the alloy substrate adopts a 304 stainless steel substrate; an additive manufacturing platform with a HWS2000 laser welding machine as the main body, the powder core wire is deposited layer by layer on the 304 stainless steel substrate at a wire feeding speed of 2 mm / s and a laser power of 1500 W to form a thin-walled wall specimen with a length, width and height ratio of approximately 75 mm×10 mm×10 mm.
[0043] Powder core wires with different WC contents were laser clad with alloy substrates of the same material to form alloy wear-resistant materials with different WC contents.
[0044] Step III, sampling the alloy wear-resistant materials with different WC contents, and conducting friction and wear tests, wear scar subsurface morphology observation, deposited structure observation, alloy hardness test and shape recovery characteristic test.
[0045] Among them, the alloy was sampled using a NSC-M332 / W6 electric spark wire cutting machine to cut friction and wear specimens and specimens for deposited structure observation with a size of 10 mm×10 mm×5 mm.
[0046] Before the friction and wear experiment, the sample surface was polished to a flat surface using 180-mesh and 400-mesh sandpaper. Subsequently, the friction and wear test was carried out on the MGW-01 reciprocating friction and wear machine. During the experiment, the sample was fixed on the device, and RHY type wheel oil was added to the sample surface. A GCr15 steel ball with a diameter of 2.1 mm was used as the friction part, the applied load was 7N, the reciprocating friction frequency was 30Hz, the stroke was 6mm, the experimental time was 60min, and the friction coefficient was automatically and dynamically collected during the experiment.
[0047] The wear scar morphology of the alloy was observed and photographed using a CMY210 optical microscope. In addition, the volume wear rate was used as a wear resistance index. The volume wear rate W s =V / d, where V is the wear volume loss and d is the sliding travel distance.
[0048] The volume wear rate was measured using a VHX-2000 confocal microscope. The wear scar depth, width and cross-sectional area at the left, middle and right sides of the wear scar were measured, and the average value of the cross-sectional area of the wear scar was taken as the volume wear rate.
[0049] The hardness of the additively manufactured alloy was measured using a HXD-1000TMB microhardness tester with a load of 0.1 kg, and the average hardness of three different areas was taken as the experimental result.
[0050] After the friction and wear experiment, the middle part of the wear scar was cut horizontally to prepare a sample for the observation of the subsurface morphology of the wear scar; the sample for observation of the deposited structure and the sample for observation of the subsurface morphology of the wear scar were prepared as metallographic samples, and after being etched by the corrosive solution, the microstructure morphology was observed by electron microscope. The composition of the corrosive solution is 3gCuSO4+10ml HCl+30ml H2O.
[0051] The bending deformation method is used to determine the shape recovery characteristics of alloy wear-resistant materials, such as Figure 7 As shown in the figure, at room temperature, the alloy sample is subjected to a predetermined deformation treatment using a bending die, that is, a 180° bend is applied to the solution-treated alloy sample using a specially designed bending die for 10 seconds. After the sample is unloaded from the die, it is left to stand at room temperature for 2 hours, during which the sample undergoes a natural recovery process of shape. The recovery angle θ of the sample after pressure unloading is measured. e and the recovery angle θ after standing for a period of time m , calculate the shape recovery rate η. It can be seen from the figure that state C is the state of the long strip sample when it is bent 180°, state B is the state of the long strip sample after pressure unloading, and state A is the state of the long strip sample after standing for a period of time; the pre-deformation ε of the sample is calculated by the sample thickness t and the mold diameter D; where:
[0052]
[0053] The shape recovery rate and the pre-deformation ε are used to evaluate the shape memory effect.
[0054] The thickness t of the long strip sample used to measure the shape recovery rate is set to 1 mm, the diameter D of the mold used is set to 25 mm, and the pre-deformation ε is calculated to be 4%.
[0055] Step IV, by comparing the results of each experiment and observation with the expected characteristics of the target material, using the W content value in step I as the end value of the new value range to narrow the value range.
[0056] Step V, repeating the above steps I to IV, wherein the WC content in step I is taken within the narrowed value range until the WC addition amount corresponding to the expected target material is obtained.
[0057] Step VI: repeat the above steps I to II according to the obtained WC addition amount to prepare an alloy wear-resistant material with expected properties.
[0058] Based on the above steps, verification is performed through an embodiment.
[0059] Example: x takes values of 0, 0.25, 0.5, 1, 2, and 4. The experimental and observed results are as follows.
[0060] In the alloy deposition morphology, such as Figure 2 As shown in , when the WC addition amount is 0.25wt.%, no obvious WC ceramic particles are observed in the alloy. It can be concluded that the added WC is completely decomposed, and its W and C elements enter the lattice gap, thereby strengthening the alloy through solid solution strengthening. As the WC content increases, since the laser parameters remain unchanged, such as power, scanning speed, defocus, powder feeding speed and other parameters, the average energy density acting on the alloy powder is fixed, so that the excessive WC hard particles are not melted, which plays a role of dispersion strengthening in the alloy; when the WC addition amount is 0.5wt.% and 1wt.%, due to the small amount of WC addition, the density of the unmelted WC hard particles in the alloy does not change significantly, resulting in the dispersion strengthening phenomenon is not significant. With the increase of WC addition; when the WC addition amount is 2wt.% and 4wt.%, the density of the unmelted WC particles increases accordingly, and the dispersion strengthening phenomenon of the WC particles begins to be significantly observed and gradually increases. As shown in Figure 3 As shown in , the appearance of Fe6W6C phase can be observed. In FeMnSi shape memory alloy, Fe6W6C can limit the movement of stacking faults, thereby inhibiting the formation of martensite, making it difficult for some austenite to transform into martensite. Therefore, with the increase of WC content, the characteristic peak of Fe6W6C phase appears and strengthens, while the peak of cooling martensite begins to weaken.
[0061] In the subsurface morphology after alloy friction and wear, such as Figure 4 As shown in the figure, the alloy with 0.5wt.% WC addition has a reduced number of martensite laths and an increased martensite spacing compared to the alloy without WC addition. When the WC content increases to 2wt.%, the number of martensite laths decreases sharply, and the martensite laths cannot be clearly observed in the figure. As the WC content increases, more Fe6W6C particles are formed in the alloy. Fe6W6C particles can limit the movement of stacking faults, resulting in a decrease in the content of cooling martensite formed in the alloy during the cooling process. These cooling martensite can provide more nucleation points for the alloy during deformation. Therefore, with the reduction of cooling martensite, the number of nucleation points of the alloy is greatly reduced, making the stress-induced martensitic phase transformation process more difficult. This phenomenon ultimately leads to a significant reduction in the number of martensitic laths, increasing the proportion of plastic deformation, and thus having an adverse effect on the shape memory properties of the alloy. In addition, during the friction and wear process, Fe6W6C particles also limit the movement of stacking faults, further limiting the formation of stress-induced martensite. This further reduces the content of stress-induced martensite in the subsurface during wear.
[0062] In terms of the memory properties of the alloy, Figure 5As shown in , the recovery rate of Fe-Mn-Si-Cr-Ni alloy without WC addition is 68.5%; when the WC addition amount is 0.25wt.%, 0.5wt.%, 1wt.%, 2wt.%, and 4wt.%, the shape recovery rates are 68.3%, 59.8%, 50.1%, 43.0%, and 38.8%, respectively. Among them, when the WC addition amount is 0.25wt.%, the WC content in the alloy is relatively small, and the W element exceeding the solid solubility limit in the alloy is limited, resulting in less Fe6W6C particles generated. It can be seen that the peak of the Fe6W6C phase is almost not observed in the XRD diagram under this condition. Therefore, the addition of 0.25wt.% WC has little effect on the shape recovery rate of the alloy, and the decline in memory performance is relatively small.
[0063] In terms of hardness and volume wear rate, such as Figure 6 As shown in the figure, with the increase of WC hard particle addition, the hardness of the alloy shows an upward trend. Among them, the hardness of the alloy without WC is about 290HV; when the addition amount of WC hard particles is 0.25wt.%, 0.5wt.%, 1wt.%, 2wt.%, and 4wt.%, the average hardness of the alloy is increased to 401, 410, 418, 459, and 458HV, respectively, which is 1.38 times, 1.41 times, 1.44 times, 1.58 times, and 1.57 times higher than the original matrix hardness.
[0064] In addition, when the addition amount of WC increases from 2wt.% to 4wt.%, under the given laser power, scanning speed, defocusing amount and powder feeding speed, the average energy density of the laser on the Fe-based alloy powder is fixed. Therefore, with the further increase in the addition amount of WC hard particles, the WC hard particles that exceed the melting capacity range cannot be effectively melted. These WC hard particles are prone to increase stress concentration, increase the possibility of cracking of the alloy, and cause defects inside the alloy, which ultimately limits the growth of the alloy hardness and causes the hardness of the alloy to no longer continue to increase.
[0065] In addition, the volume wear rates of the alloys without WC addition and with 0.25wt.%, 0.5wt.%, 1wt.%, 2wt.%, and 4wt.% WC addition were 24444, 19875, 34761, 48160, 35138, and 28710×10 -6 mm 3 / mm. According to the above volume wear rate, compared with the alloy without WC, the wear resistance of the alloy with 0.25wt.% WC increased by 23.1%, the wear resistance of the alloy with 0.5wt.% WC decreased by 29.7%, the wear resistance of the alloy with 1wt.% WC decreased by 49.2%, the wear resistance of the alloy with 2% WC decreased by 30.4%, and the wear resistance of the alloy with 4wt.% WC decreased by 14.8%. It can be seen that the volume wear rate of the alloy shows a trend of first decreasing, then increasing, and then decreasing, and reaches the lowest point when 0.25wt.% WC is added.
[0066] The above description is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the above principles of the present invention. These improvements and modifications are also considered to be within the scope of protection of the present invention.
Claims
1. Alloy wear-resistant material with wear resistance adjusted based on WC content, characterized by: It is prepared by laser fuse deposition additive manufacturing and is marked as matrix-xWC alloy wear-resistant material, wherein the material matrix is an iron-based shape memory alloy, x is the value of the WC addition in the alloy wear-resistant material, x∈[0.25,4]; when the WC addition is 0.25-1wt.%, the wear resistance of the alloy wear-resistant material shows a downward trend; when the WC addition is 1-4wt.%, the wear resistance of the alloy wear-resistant material shows an upward trend.
2. The alloy wear-resistant material according to claim 1, characterized in that: The material matrix is Fe-Mn-Si-Cr-Ni alloy, and the prepared alloy wear-resistant material is marked as Fe-Mn-Si-Cr-Ni-xWC alloy, x∈[0.25,4], among which the Fe-Mn-Si-Cr-Ni-0.25WC alloy wear-resistant material has the highest wear resistance.
3. The alloy wear-resistant material according to claim 2, characterized in that: When the WC addition amount is 0.25wt.%, there are no obvious WC particles in the alloy deposition morphology. As the WC addition amount increases, the WC particle density increases.
4. The alloy wear-resistant material according to claim 3, characterized in that: When 0.25-1wt.% WC is added, the added WC decomposes and the released tungsten element is partially dissolved in the material matrix. The tungsten element exceeding the solid solubility limit reacts with iron and carbon elements to generate Fe6W6C type carbides.
5. The alloy wear-resistant material according to claim 4, characterized in that: When 0.25-1wt.% WC is added, as the WC content increases, in the sub-surface morphology of the alloy wear-resistant material after friction and wear, the number of martensite laths decreases and the spacing between martensite increases; wherein, the increase in WC content leads to an increase in the content of Fe6W6C, and the Fe6W6C carbide particles hinder the sliding of the slip band of the material matrix, which is used to inhibit the formation of martensite and hinder the positive phase transformation of part of austenite to martensite, so as to weaken the unique friction reduction and wear resistance of the material matrix.
6. The alloy wear-resistant material according to claim 5, characterized in that: When 1-4wt.% WC is added, undissolved WC hard particles appear, and as the WC content increases, the density of WC hard particles in the alloy wear-resistant material increases.
7. The alloy wear-resistant material according to claim 6, characterized in that: When 0.25-4wt.% WC is added, the memory property of the alloy wear-resistant material gradually decreases as the content of WC increases.
8. The alloy wear-resistant material with wear resistance adjusted based on WC content according to claim 7, characterized in that: When 0.25-2wt.% WC is added, the hardness of the alloy wear-resistant material increases as the content of WC increases; when 2-4wt.% WC is added, the hardness of the alloy wear-resistant material remains unchanged.
9. The method for preparing an alloy wear-resistant material according to any one of claims 1 to 8, characterized in that: The following steps are involved: Step I, preparing a powder core wire, wrapping a mixed alloy powder with an alloy tube as an outer skin, and drawing to form a wire material with uniform diameter; the main components of the powder core wire are Fe, Mn, Si, Cr, Ni and WC; wherein, the same material alloy outer skin a is used and mixed alloy powder b with different WC content is used to prepare powder core wires with various WC contents, and the WC content is within the range of 0.25-4wt.%; Step II, using laser cladding technology, feeding the powder core wire to the alloy substrate at a uniform speed, and stacking layer by layer to form a thin-wall coating to form an alloy wear-resistant material; wherein the powder core wires with different WC contents are laser clad with the alloy substrate of the same material to form alloy wear-resistant materials with different WC contents; Step III, sampling the alloy wear-resistant materials with different WC contents, and conducting friction and wear tests, wear scar subsurface morphology observation, deposited structure observation, alloy hardness test and shape recovery characteristic test respectively; Step IV, by comparing the results of each experiment and observation with the expected characteristics of the target material, using the W content value in step I as the end value of the new value range to narrow the value range; Step V, repeating the above steps I to IV, wherein the amount of WC added in step I is taken within the reduced value range until the WC content corresponding to the expected target material is obtained; Step VI: repeat the above steps I to II according to the obtained WC addition amount to prepare an alloy wear-resistant material with expected properties.
10. The method for preparing an alloy wear-resistant material with wear resistance adjusted based on WC content according to claim 9, characterized in that: After the friction and wear experiment, the middle part of the wear scar was horizontally cut into samples for observation of the subsurface morphology of the wear scar. The samples for observation of the deposited structure and the subsurface morphology of the wear scar were prepared into metallographic samples, and after being etched by the corrosive liquid, the microstructure morphology was observed by electron microscope. The bending deformation method was used to determine the shape recovery characteristics of the alloy wear-resistant material. Under normal temperature conditions, the alloy sample was subjected to a predetermined deformation treatment using a bending die. After standing for a period of time, the recovery angle θ of the sample after pressure unloading was measured. e and the recovery angle θ after standing for a period of time m , calculate the shape recovery rate η; calculate the pre-deformation ε of the sample by the sample thickness t and the mold diameter D; where: The shape recovery rate η and the pre-deformation amount ε are used to evaluate the shape memory effect.