Preparation process of high-performance lens array film

Through the combined process of ultrasonic cleaning and PVD thermal vapor deposition film, the problem of insufficient edge barrier accuracy in the coating area in the lens array film is solved, and high-precision lens array film preparation is achieved, ensuring the stability and cleanliness of the coating layer.

CN118932292APending Publication Date: 2024-11-12苏州东辉光学有限公司
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411000151.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art is difficult to achieve high-precision coating area edge barriers in lens array films, especially when the distance between lenses is only 0.5mm in the new design scheme, the coating area edge barriers are difficult to achieve the requirement of less than 0.2mm.

Method used

The high-performance lens array film preparation process using ultrasonic cleaning tooling combined with PVD hot steaming method is used to ensure the cleanliness of the lens surface and coating accuracy through multi-step ultrasonic cleaning and vacuum coating machine. The specific steps include multiple ultrasonic cleaning and drying treatments, and then setting the appropriate vacuum degree, temperature and gas flow rate in the vacuum coating machine to achieve high-precision coating.

Benefits of technology

Through high-clean cleaning steps and high-precision coating process, the surface cleanliness and reliability of the coating layer are ensured, and the edge barrier of the high-precision coating area is achieved, which avoids the problem of coating layer falling off caused by impurities, and meets the new design plan. High precision requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932292A_ABST
    Figure CN118932292A_ABST
Patent Text Reader

Abstract

The invention discloses a high-performance lens array film preparation process which comprises the following steps: providing a cleaning tool, and placing a to-be-cleaned lens in the cleaning tool for ultrasonic cleaning; the cleaned lens is placed in a film coating tool; and a PVD thermal evaporation mode is adopted for coating according to preset film type parameters. Through the high-cleanliness cleaning step, the surface of the workpiece to be coated is fully cleaned, high cleanliness is guaranteed, and the situation that a coating layer is low in reliability and prone to falling off due to impurities or particles after the surface of the workpiece is coated is avoided. And under the auxiliary action of the film coating tool, high-precision film coating area edge blocking can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of thin film preparation, and in particular to a process for preparing a high-performance lens array thin film. Background Art

[0002] As a special material form, optical and optoelectronic films have now widely penetrated into various new scientific and technological fields. In particular, in recent years, the development and application of various special properties of the rapidly developing and eye-catching thin film photonic crystals, quantum dot films, multi-dimensional structures at nanometer or sub-wavelength scales, ferroelectric nonlinear films with high electro-optic coefficients, photorefractive films, photon detection films, sensor function films, high-density volume recording films and organic light-emitting display films, etc., are all related to the characteristics of optical films. This is why optical films have developed rapidly in recent years. Because of their good spatial periodic structure, it is easy to carry out complex artificial tailoring and design of the structure, components and properties of the film based on the theory of optical films, thereby achieving excellent performance that other technologies cannot achieve.

[0003] PEI is a non-crystalline plastic, an amorphous high-performance polymer. It is an engineering plastic made of amorphous Lens array (polyetherimide) and extruded at high temperature by an extruder. The long-term creep resistance of polyetherimide under high temperature and stress allows it to replace metal and other materials in many structural devices. It exhibits good electrical properties under variable temperature, humidity and frequency conditions.

[0004] In the industry, Lens array is a light-transmitting component with complex structure, small size and 1mm distance between lenses in the light-transmitting area. However, the distance between lenses in the new design is only 0.5mm. The coating edge of the light-transmitting area should be less than 0.2mm, while the conventional tooling design can only achieve an edge of less than 1mm.

[0005] Therefore, a high-performance lens array thin film preparation process is still needed to solve the above problems. Summary of the invention

[0006] The present invention provides a high-performance lens array film preparation process for solving the above-mentioned problem.

[0007] The purpose of the present invention is achieved by the following technical solutions:

[0008] A high-performance lens array thin film preparation process, comprising:

[0009] Providing a cleaning tool, placing the lens to be cleaned in the cleaning tool and cleaning it with ultrasonic wave;

[0010] Placing the cleaned lens in a coating tool;

[0011] The PVD thermal evaporation method is used to coat the film according to the preset film parameters.

[0012] In one embodiment, placing the lens to be cleaned in the cleaning tool and cleaning it with ultrasonic wave comprises:

[0013] a: placing the lens in the cleaning tool and cleaning it in a cleaning agent with a pH of 8, an ultrasonic power of 28KHz, and a temperature of 50°C for 10 minutes;

[0014] b: The lenses after preliminary cleaning are transferred to a cleaning agent at a temperature of 50° C. through a cleaning tool, and cleaned for 5 minutes at an ultrasonic power of 40 KHz;

[0015] c: then place the lens in pure water at 45°C and clean it for 5 minutes with an ultrasonic power of 40KHz;

[0016] d: then placing the lens in a cleaning solution at a temperature of 45° C. and a pH of 7, and cleaning it at an ultrasonic power of 68 KHz for 5 minutes;

[0017] e: The lens is then placed in pure water at a temperature of 45°C and cleaned for 5 minutes using an ultrasonic power of 40KHz;

[0018] f: Then place the lens in pure water and rinse at 40KHz, and finally turn off the ultrasound, lift the lens and use gravity to remove moisture, so that the humidity value on the lens surface is less than 0.02%, and use an oven to dry at 50-55°C for 4 hours.

[0019] In one embodiment, the cleaning tool comprises:

[0020] A tooling seat, wherein a plurality of workstations for placing products to be coated are arranged on the tooling seat, a stopper is arranged on the workstation, the stopper is arranged between two adjacent workstations and is used to stop at least one side of the product, a limiting member is arranged on the workstation, the limiting member is used to stop at least one side of the product, and a coating port for exposing a portion of the channel on the product is opened at the bottom of the workstation;

[0021] The blocking knife is connected to the bottom strip groove of the tooling seat, corresponding to the coating opening, and can be moved along the width direction of the strip groove to cover the coating opening on some products.

[0022] In one embodiment, the method of coating a film according to preset film parameters by PVD thermal evaporation includes:

[0023] Pre-process: provide a vacuum coating machine, set the vacuum degree to 8×10-4pa, the coating evaporation temperature to 50℃, BV to 500V, BmA to 450mA, and ACC to 400V; let oxygen enter the vacuum coating machine at a flow rate of 50sccm, gas one enters the vacuum coating machine at a flow rate of 40sccm, and gas two enters the vacuum coating machine at a flow rate of 10sccm.

[0024] In one embodiment, a vapor deposition process is further included after the pre-process, and the vapor deposition process includes:

[0025] Set the BV of TA2O5 to 500V, BmA to 450mA, and ACC to 400V. Oxygen enters the vacuum coating machine at a flow rate of 50sccm, gas one at 40sccm, and gas two at 10sccm.

[0026] Set the BV of SIO2 to 600V, BmA to 500mA, and ACC to 400V. Oxygen enters the vacuum coating machine at a flow rate of 5sccm, gas one is blown in at 40sccm, and gas two is blown in at 10sccm.

[0027] In one embodiment, the current for evaporating TA2O5 is 250 mA and the rate is 0.2 nm / s;

[0028] The current for evaporating SiO2 is 150mA and the rate is 0.65nm / s; the current for evaporating CR is 50mA and the rate is 0.5nm / s.

[0029] In one embodiment, the vacuum degree of evaporating TA2O5 is 2×10 -2 Pa, the vacuum degree of evaporating SiO2 is 1.6×10 -2 Pa, the vacuum degree of evaporation CR is 9×10 -4 Pa.

[0030] In one embodiment, a connecting hole is provided at the bottom of the tooling seat, and a strip hole is provided on the knife block, and the knife block is attached to the bottom of the tooling seat by bolt connection.

[0031] Compared with the prior art, the beneficial effects of the present invention include at least:

[0032] Through the high-clean cleaning steps, the surface of the workpiece to be coated is fully cleaned to ensure a high degree of cleanliness, avoiding impurities or particles on the surface of the workpiece after coating, resulting in low reliability of the coating layer and easy falling off. And with the assistance of the coating tooling, high-precision coating area ribs can be achieved. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 Schematic diagram of the preparation process of an embodiment of the present invention;

[0034] Figure 2 2 is a schematic diagram of the coating tooling structure of an embodiment of the present invention;

[0035] Figure 3 is a micrograph 1 of embodiment 2 of the present invention;

[0036] Figure 4 is a second micrograph of the second embodiment of the present invention;

[0037] Figure 5 is a micrograph 3 of embodiment 2 of the present invention;

[0038] Figure 6 is a micrograph 1 of embodiment 1 of the present invention;

[0039] Figure 7 FIG2 is a micrograph of an embodiment of the present invention.

[0040] In the figure: 1. tooling seat; 2. knife stopper; 3. connecting hole; 4. strip hole; 5. bolt; 14. strip groove. DETAILED DESCRIPTION

[0041] Example embodiments will now be described more fully with reference to the accompanying drawings. However, example embodiments can be implemented in a variety of forms and should not be construed as limited to the embodiments set forth herein; rather, these embodiments are provided to make the present invention more comprehensive and complete and to fully convey the concepts of example embodiments to those skilled in the art. The same reference numerals in the figures represent the same or similar structures, and thus their repeated description will be omitted.

[0042] The words expressing positions and directions described in the present invention are all explained with reference to the accompanying drawings as examples, but they can be changed as needed, and all such changes are included in the protection scope of the present invention.

[0043] The present invention provides a high-performance lens array thin film preparation process, comprising:

[0044] A cleaning tool is provided, and the lens to be cleaned is placed in the cleaning tool for ultrasonic cleaning. With the assistance of the cleaning tool, the surface of the lens is cleaned.

[0045] In one embodiment, placing the lens to be cleaned in the cleaning tool and cleaning it with ultrasonic wave comprises:

[0046] a: Place the lens in the cleaning tool and clean it in a cleaning solution with a pH of 8, an ultrasonic power of 28KHz, and a temperature of 50°C for 10 minutes. Immerse the lens in the cleaning tool in an alkaline liquid with a pH of 8, and then use an ultrasonic cleaning method with a power of 28KHz for 10 minutes to fully clean the dust, dirt or impurities on the surface of the lens.

[0047] b: The lenses after preliminary cleaning are transferred to a cleaning agent at a temperature of 50°C through a cleaning tool, and cleaned for 5 minutes at an ultrasonic power of 40KHz. The lenses after preliminary cleaning are transferred to a cleaning pool at an ultrasonic power of 40KHz, for example, by rinsing with clean water for 5 minutes to remove the impurities remaining on the lenses again.

[0048] c: Place the lens in pure water at 50°C and clean it for 5 minutes with an ultrasonic power of 40KHz. After cleaning, change the lens to another cleaning agent with the same conditions for cleaning. Avoid incomplete cleaning with the cleaning agent in step a, which will affect the subsequent formation of a stable coating layer.

[0049] d: Then the lens is placed in a cleaning agent at a temperature of 45°C and a pH of 7, and cleaned for 5 minutes at an ultrasonic power of 68KHz. Then the lens after step c is transferred to a cleaning agent at a pH of 7, and then the lens is fully cleaned at an ultrasonic power of 68KHz.

[0050] e: Place the lens in pure water at a temperature of 45°C and clean it for 5 minutes at an ultrasonic power of 40KHz. Place the lens in step d in pure water again and clean the impurities on the surface of the lens at an ultrasonic power of 40KHz.

[0051] f: Then place the lens in pure water and rinse it at 40KHz, and finally turn off the ultrasound, lift the lens and use gravity to remove moisture, so that the humidity value on the lens surface is less than 0.02%, and use an oven to dry it at 50-55°C for 4 hours. Through multiple steps, the lens is fully cleaned, and after cleaning, gravity is used to remove moisture, so that the surface of the lens is in a relatively dry state, and the humidity value is less than 0.02%. Finally, the oven is used to provide a temperature of 50-55°C, and the surface of the lens is dried for four hours to complete the full drying of the surface. Provide a stable and clean lens surface for subsequent coating. Avoid unreliable bonding between the coating layer and the lens due to the presence of impurities between the coating layer and the lens.

[0052] The cleaned lens is placed in a coating tool.

[0053] The PVD thermal evaporation method is used to coat the film according to the preset film parameters.

[0054] The method of coating according to preset film parameters by PVD thermal evaporation includes:

[0055] Pre-process: Provide vacuum coating machine, set the vacuum degree to 8×10 -4 Pa, the coating evaporation temperature is 55°C, BV is 500V, BmA is 450mA, and ACC is 400V. The model of the vacuum coating machine is OTFC-1300. Before coating, the vacuum degree inside the cavity of the vacuum coating machine is 8×10 -4 Pa. The coating distillation temperature is set to 50°C, and the temperature inside the vacuum coating machine is set to 50°C.

[0056] Oxygen is introduced into the vacuum coating machine at a flow rate of 50sccm, gas one is introduced into the vacuum coating machine at a flow rate of 40sccm, and gas two is introduced into the vacuum coating machine at a flow rate of 10sccm. During preheating, oxygen, gas one and gas two are first blown into the vacuum coating machine at the above flow rates. The vacuum coating machine is put into reaction conditions in advance, and both gas one and gas two are argon, so that the inside of the vacuum coating machine is filled with protective gas to avoid external gas pollution. Argon is mainly used for auxiliary heating, atmosphere protection and cooling of electron beams and ion beams.

[0057] In one embodiment, a vapor deposition process is further included after the pre-process, and the vapor deposition process includes: setting the BV of TA2O5 to 500V, the BmA to 450mA, and the ACC to 400V, oxygen is introduced into the vacuum coating machine at a flow rate of 50sccm, gas one is blown in at 40sccm, and gas two is blown in at 10sccm;

[0058] Set the BV of SIO2 to 600V, BmA to 500mA, and ACC to 400V. Oxygen enters the vacuum coating machine at a flow rate of 5sccm, gas one at 40sccm, and gas two at 10sccm.

[0059] Preferably, the current for evaporating TA2O5 is set to 250 mA and the rate is 0.2 nm / s;

[0060] The current for evaporating SiO2 is 150mA and the rate is 0.65nm / s; the current for evaporating CR is 50mA and the rate is 0.5nm / s.

[0061] The vacuum degree of evaporating TA2O5 is 2×10 -2 Pa, the vacuum degree of evaporating SiO2 is 1.6×10 -2 Pa, the vacuum degree of evaporation CR is 9×10 -4 Pa.

[0062] Among them, the cleaning tooling includes:

[0063] A tooling seat 1 is provided with a plurality of workstations for placing products to be coated, a stopper is provided on the workstation, the stopper is provided between two adjacent workstations and is used to stop at least one side of the product, a limiter is provided on the workstation and is used to stop at least one side of the product, and a coating port for exposing a channel on a part of the product is provided at the bottom of the workstation. The tooling seat 1 can be connected to the top of the evaporation chamber inside the vacuum coating machine.

[0064] The knife block 2 is connected to the bottom strip groove 14 of the tooling seat 1, corresponding to the coating port, and can be moved along the width direction of the strip groove 14 to block the coating port on part of the product. The knife block 2 is slidably connected to the tooling seat 1. When adjusting, the knife block 2 can be manually adjusted to move horizontally along the width direction of the strip groove 14, so that the projection position of the knife block 2 on the product moves relatively. Therefore, when coating, by moving the lateral position of the knife block 2 in the strip groove 14, it is possible to accurately control the blocking of the light-transmitting compartments with extremely small spacing on the product, and perform coating and non-coating respectively, to meet the actual process requirements.

[0065] In one embodiment, the bottom of the tooling seat 1 is provided with a connection hole 3, and the knife block 2 is provided with a strip hole 4, and the knife block 2 is connected and attached to the bottom of the tooling seat 1 through a bolt 5. The knife block 2 can achieve precise control of the shielding distance through the cooperation of the strip hole 4 and the bolt 5.

[0066] Embodiment 1:

[0067] Product 1 is successively passed through an alkaline solution with a pH of 8 and a temperature of 50S°C, cleaned for 10 minutes at an ultrasonic power of 28KHz, and then the product is transferred again to a cleaning agent solution of win 213C - Mountain Wind at a temperature of 50°C and cleaned for 5 minutes at an ultrasonic power of 40KHz. Then the product is transferred to pure water at 50 degrees Celsius and cleaned for 5 minutes at an ultrasonic power of 40KHz. Then the product is transferred to a cleaning agent solution of win 213C - Mountain Wind with a pH of 8 and cleaned for 5 minutes at an ultrasonic power of 68KHz. Then the product is transferred to pure water at 50°C and cleaned for 5 minutes at an ultrasonic power of 40KHz. Finally, the water is removed by gravity settling and dried in an oven at 55°C for 4 hours. Then, the product is placed into a coating optical thin film machine OTFC - 1300 by the carrying of the tooling seat 1, and the vacuum degree is set to 8×10-4Pa, the coating evaporation temperature is 80°C, BV is 500V, BmA is 450mA, ACC is 400V;, then oxygen enters the vacuum coating machine at a flow rate of 50sccm, oxygen 1 enters the vacuum coating machine at a flow rate of 40sccm, and argon 2 enters the vacuum coating machine at a flow rate of 10sccm. Then, the BV of TA2O5 is set to 500V, BmA is 450mA, ACC is 400V; the BV of SIO2 is set to 600V, BmA is 500mA, ACC is 400V, oxygen enters the vacuum coating machine at a flow rate of 5sccm, gas 1 enters at 40sccm, and gas 2 enters at 10sccm. The current for evaporating TA2O5 is 250mA and the rate is 0.2nm / s;

[0068] The current for evaporating SiO2 is 150mA and the rate is 0.65nm / s; the current for evaporating CR is 50mA and the rate is 0.5nm / s.

[0069] The film layer prepared on the workpiece in Example 1 is detected:

[0070] 1. Appearance detection: The film layer has no demolding, bubbling, and film cracking.

[0071] 2. Adhesion test: Boil for 2H, use 3M tape to quickly pull the film layer 5 times along a direction nearly 90° to the film layer, and the film layer has no film peeling, bubbling, and film cracking.

[0072] 3. Rubbing test: Rub the film layer surface 10 times with a force of about 1 pound, and the film layer has no film peeling, bubbling, and film cracking.

[0073] Example 2:

[0074] Product 2 is sequentially washed with alkali solution of pH 8 and temperature 50 at 60KHz ultrasonic power for 10 minutes, then transferred to a pure water pool for washing at 60KHz ultrasonic power for 50 minutes, and finally allowed to stand by gravity to remove moisture, and dried in an oven at 55°C for 4 hours. Then the product is placed in the coating machine OTFC-1300 by the tooling seat 1, and the vacuum degree is set to 8×10-4Pa, the coating evaporation temperature is 50°C, the BV is 500V, the BmA is 450mA, and the ACC is 400V. Then oxygen is introduced into the vacuum coating machine at a flow rate of 50sccm, oxygen 1 is introduced into the vacuum coating machine at a flow rate of 40sccm, and argon 2 is introduced into the vacuum coating machine at a flow rate of 10sccm. Then the BV, BmA and ACC of TA2O5 are set to 500V, 450mA and 400V. Oxygen enters the vacuum coating machine at a flow rate of 50 sccm, gas 1 at 40 sccm, and gas 2 at 10 sccm. The current for evaporating TA2O5 is 250 mA, and the rate is 0.2 nm / s;

[0075] Set the BV of SIO2 to 600V, BmA to 500mA, ACC to 400V, oxygen to enter the vacuum coating machine at a flow rate of 5sccm, gas 1 to 40sccm, and gas 2 to 10sccm. The current for evaporating TA2O5 is 250mA, and the rate is 0.2nm / s;

[0076] The current for evaporating SiO2 is 150mA and the rate is 0.65nm / s; the current for evaporating CR is 50mA and the rate is 0.5nm / s.

[0077] The film layer prepared on the workpiece in Example 2 was tested:

[0078] 1. Appearance inspection: The film layer has slight demoulding, bubbling and film cracking.

[0079] 2. Adhesion test: Boil in water for 2 hours and use 3M tape to quickly pull the film layer 5 times in a direction close to 90° to the film layer. The film layer will peel off, bubble, and crack.

[0080] 3. Rub test: Rub the film surface 10 times with a force of about 1 pound, and the film will be completely peeled off.

[0081] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. A person skilled in the art may change, modify, substitute and modify the above embodiments within the scope of the invention without departing from the principles and purpose of the present invention. All such changes should fall within the scope of protection of the claims of the present invention.

Claims

1. A high-performance lens array thin film preparation process, characterized in that: include: Providing a cleaning tool, placing the lens to be cleaned in the cleaning tool and cleaning it with ultrasonic wave; Placing the cleaned lens in a coating tool; The PVD thermal evaporation method is used to coat the film according to the preset film parameters.

2. The high performance lens array thin film preparation process according to claim 1, characterized in that: Placing the lens to be cleaned in the cleaning tool and cleaning it with ultrasonic wave comprises: a: placing the lens in the cleaning tool and cleaning it in a cleaning agent with a pH of 8, an ultrasonic power of 28KHz, and a temperature of 50°C for 10 minutes; b: The lenses after preliminary cleaning are transferred to a cleaning agent at a temperature of 50° C. through a cleaning tool, and cleaned for 5 minutes at an ultrasonic power of 40 KHz; c: then placing the lens in pure water at 45°C and cleaning it with an ultrasonic power of 40KHz for 5 minutes; d: Then the lens is placed in a cleaning agent at a temperature of 45° C. and a pH of 7, and cleaned at an ultrasonic power of 68 KHz for 5 minutes; e: placing the lens in pure water at a temperature of 45°C and cleaning it with an ultrasonic power of 40KHz for 5 minutes; f: Then place the lens in pure water and rinse at 40KHz, and finally turn off the ultrasound, lift the lens and use gravity to remove moisture, so that the humidity value on the lens surface is less than 0.02%, and use an oven to dry at 50-55°C for 4 hours.

3. The high performance lens array thin film preparation process according to claim 2, characterized in that: The cleaning tool comprises: A tooling seat, wherein a plurality of workstations for placing products to be coated are arranged on the tooling seat, a stopper is arranged on the workstation, the stopper is arranged between two adjacent workstations and is used to stop at least one side of the product, a limiting member is arranged on the workstation, the limiting member is used to stop at least one side of the product, and a coating port for exposing a portion of the channel on the product is opened at the bottom of the workstation; The blocking knife is connected to the bottom strip groove of the tooling seat, corresponding to the coating opening, and can be moved along the width direction of the strip groove to cover the coating opening on some products.

4. The high performance lens array thin film preparation process according to claim 1, characterized in that: The method of coating according to preset film parameters by PVD thermal evaporation includes: Pre-process: Provide vacuum coating machine, set the vacuum degree to 8×10 -4 Pa, the coating evaporation temperature is 55°C, BV is 500V, BmA is 450mA, and ACC is 400V; Oxygen is introduced into the vacuum coating machine at a flow rate of 50 sccm, gas one is introduced into the vacuum coating machine at a flow rate of 40 sccm, and gas two is introduced into the vacuum coating machine at a flow rate of 10 sccm.

5. The high performance lens array thin film preparation process according to claim 4, characterized in that: It also includes a vapor deposition process after the pre-process, and the vapor deposition process includes: Set the BV of TA2O5 to 500V, BmA to 450mA, and ACC to 400V. Oxygen enters the vacuum coating machine at a flow rate of 50sccm, gas one at 40sccm, and gas two at 10sccm. Set the BV of SIO2 to 600V, BmA to 500mA, and ACC to 400V. Oxygen enters the vacuum coating machine at a flow rate of 5sccm, gas one at 40sccm, and gas two at 10sccm.

6. The high performance lens array thin film preparation process according to claim 5, characterized in that: The current for evaporating TA2O5 was 250 mA and the rate was 0.2 nm / s; The current for evaporating SiO2 is 150mA and the rate is 0.65nm / s; the current for evaporating CR is 50mA and the rate is 0.5nm / s.

7. The high performance lens array thin film preparation process according to claim 6, characterized in that: The vacuum degree of evaporating TA2O5 is 2×10 -2 Pa, the vacuum degree of evaporating SiO2 is 1.6×10 -2 Pa, the vacuum degree of evaporation CR is 9×10 -4 Pa.

8. The high performance lens array thin film preparation process according to claim 3, characterized in that: The bottom of the tooling seat is provided with a connecting hole, and the knife blocks are provided with strip holes. The knife blocks are connected and attached to the bottom of the tooling seat by bolts.

Citation Information