Method for preparing lithium hydroxide from aluminum-based lithium concentrate

By using inorganic acid leaching and bipolar membrane electrolysis in aluminum-based lithium concentrate, the complete process flow from aluminum-based lithium concentrate to lithium hydroxide is achieved, and the problem of failure to effectively utilize lithium resources is solved. High purity and efficient lithium hydroxide products.

CN118932346APending Publication Date: 2024-11-12ZHENGZHOU NON FERROUS METALS RES INST CO LTD OF CHALCO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411112031.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art does not involve a complete process flow from aluminum-based lithium concentrate to lithium hydroxide products, resulting in the failure of effective utilization of lithium resources.

Method used

By mixing aluminum-based lithium concentrate with inorganic acid for leaching, then solid-liquid separation and pH adjustment, purifying with ion exchange resin, and finally bipolar membrane electrolysis to obtain a high-purity lithium hydroxide solution and crystallization by evaporation to obtain Lithium hydroxide products, and inorganic acids can be returned to the process for leaching lithium concentrate, achieving efficient utilization.

Benefits of technology

It realizes efficient lithium extraction in aluminum-based lithium concentrate, with a leachate rate of more than 98%, removes impurities and ions, and obtains lithium hydroxide products with a purity of ≥99.5%, simplifies the process, reduces energy consumption, and solves the failure of lithium resources. Issues of effective utilization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932346A_ABST
    Figure CN118932346A_ABST
Patent Text Reader

Abstract

The invention relates to a method for preparing lithium hydroxide from aluminum-based lithium concentrate. The method comprises the following steps: obtaining aluminum-based lithium concentrate slurry; leaching the aluminum-based lithium concentrate slurry by using an inorganic acid, and then carrying out solid-liquid separation to obtain a lithium-removed slag filter cake and a lithium salt solution; adjusting the pH value of the lithium salt solution, and then performing refined filtration to obtain a refined filtrate; purifying the fine filtrate by using ion exchange resin to obtain a lithium salt pre-electrolyte; performing bipolar membrane electrolysis on the lithium salt pre-electrolyte to obtain a lithium hydroxide solution and inorganic acid; evaporating and concentrating the lithium hydroxide solution to obtain a lithium hydroxide product; wherein the purity of the lithium hydroxide product is greater than or equal to 99.5%; and the inorganic acid can be returned to the process for leaching the lithium concentrate after the concentration is adjusted, so that efficient and full-quantitative utilization of the aluminum-based lithium concentrate is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium salt preparation, and in particular to a method for preparing lithium hydroxide from aluminum-based lithium concentrate. Background Art

[0002] As one of the three basic lithium salts in the lithium industry chain, lithium hydroxide is an important raw material for manufacturing power batteries, glass, ceramics and other products. High-nickel ternary cathode materials prepared with lithium hydroxide as raw material have the advantages of low sintering temperature, good cycle stability, and strong high-voltage resistance. With the development trend of high-nickel ternary cathode materials for power batteries, the demand for lithium hydroxide is increasing year by year.

[0003] my country is rich in lithium resources associated with sedimentary bauxite. The Li2O content in bauxite is usually between 0.015% and 0.2%, and the average content in the advantageous mining section can reach more than 0.1%. The resource volume exceeds 2 million tons (Li2O), which is a potential super-large lithium resource library. The lithium extraction technology currently developed in the alumina production process can stably and efficiently produce aluminum-based lithium concentrate from the alumina production process. The development and preparation of lithium products based on aluminum-based lithium concentrate can not only reduce the lithium content in alumina products and eliminate the adverse effects on downstream aluminum electrolysis enterprises, but also improve my country's lithium strategic resource guarantee capabilities and realize the independent control of lithium salt basic raw materials. It is of great significance. However, the complete process from aluminum-based lithium concentrate to lithium hydroxide products is not currently involved. Summary of the invention

[0004] The present application provides a method for preparing lithium hydroxide from aluminum-based lithium concentrate to solve the following technical problem: how to prepare lithium hydroxide from aluminum-based lithium concentrate.

[0005] In a first aspect, the present application provides a method for preparing lithium hydroxide from aluminum-based lithium concentrate, the method comprising:

[0006] Obtaining aluminum-based lithium concentrate slurry;

[0007] The aluminum-based lithium concentrate slurry is leached using an inorganic acid, and then solid-liquid separation is performed to obtain a lithium-removed slag filter cake and a lithium salt solution;

[0008] The lithium salt solution is subjected to pH adjustment and then fine filtration to obtain a fine filtrate;

[0009] Purifying the refined filtrate using an ion exchange resin to obtain a lithium salt pre-electrolyte;

[0010] The lithium salt pre-electrolyte is subjected to bipolar membrane electrolysis to obtain a lithium hydroxide solution and an inorganic acid.

[0011] Optionally, the aluminum-based lithium concentrate slurry is obtained, comprising:

[0012] The aluminum-based lithium concentrate is mixed with water to obtain an aluminum-based lithium concentrate slurry; wherein the median particle size of the aluminum-based lithium concentrate is 30 μm to 60 μm, and the solid content of the aluminum-based lithium concentrate slurry is 200 g / L to 600 g / L.

[0013] Optionally, the inorganic acid includes at least one of the following: nitric acid and sulfuric acid.

[0014] Optionally, the amount of the inorganic acid used is 0.05% to 5% by weight of the aluminum-based lithium concentrate slurry.

[0015] Optionally, the leaching process parameters include: temperature of 40°C to 80°C, and time of 0.5h to 3h.

[0016] Optionally, the target pH of the pH adjustment is 7-12.

[0017] Optionally, in the refined filtrate, the concentration of lithium ions is 0.1 g / L to 2 g / L, and the concentration of aluminum ions is ≤5 mg / L.

[0018] Optionally, the Ca in the lithium salt pre-electrolyte 2+ With Mg 2+ The mixed ion concentration is ≤2mg / L.

[0019] Optionally, the median particle size of the lithium-removing slag filter cake is 5 μm to 30 μm.

[0020] Optionally, the method further includes:

[0021] The lithium hydroxide solution is evaporated and concentrated to obtain a lithium hydroxide product; wherein the purity of the lithium hydroxide product is ≥99.5%.

[0022] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0023] The method for preparing lithium hydroxide from aluminum-based lithium concentrate provided in the embodiment of the present application comprises: obtaining aluminum-based lithium concentrate slurry; leaching the aluminum-based lithium concentrate slurry with an inorganic acid, and then performing solid-liquid separation to obtain a lithium-free slag filter cake and a lithium salt solution; adjusting the pH of the lithium salt solution, and then performing fine filtration to obtain a fine filtrate; purifying the fine filtrate with an ion exchange resin to obtain a lithium salt pre-electrolyte; and performing bipolar membrane electrolysis on the lithium salt pre-electrolyte to obtain a lithium hydroxide solution and an inorganic acid. 12 · Lithium in the form of 3H2O can be leached to achieve efficient extraction of lithium from aluminum-based lithium concentrate. The leaching rate of aluminum-based lithium concentrate can reach more than 98%. At the same time, CO3 can also be effectively removed from aluminum-based lithium concentrate slurry. 2- , thereby preventing Li in aluminum-based lithium concentrate slurry+ With CO3 2- The reaction occurs and precipitates in advance; after solid-liquid separation, pH adjustment and fine filtration, the impurity ions in the slurry after leaching can be removed to a large extent, so that a pure fine filtrate containing lithium ions can be obtained; the lithium salt pre-electrolyte is subjected to bipolar membrane electrolysis, and the products are lithium hydroxide solution and inorganic acid. The lithium hydroxide solution can be evaporated and crystallized to obtain a lithium hydroxide product with a purity of ≥99.5%, and the inorganic acid can be returned to the process after adjusting the concentration for leaching lithium concentrate, thereby realizing efficient and full-quantity utilization of aluminum-based lithium concentrate. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0025] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0026] Figure 1 A schematic flow chart of a method for preparing lithium hydroxide from an aluminum-based lithium concentrate provided in an embodiment of the present application;

[0027] Figure 2 A schematic diagram of the actual process of a method for preparing lithium hydroxide from an aluminum-based lithium concentrate provided in an embodiment of the present application. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0029] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0030] In the present application, the terms "include", "comprising", etc. mean "including but not limited to". "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or plural, respectively.

[0031] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0032] In a first aspect, the present application provides a method for preparing lithium hydroxide from aluminum-based lithium concentrate. Figure 1 A schematic diagram of a process for preparing lithium hydroxide from an aluminum-based lithium concentrate provided in an embodiment of the present application; see Figure 1 , the method comprising:

[0033] In a first aspect, the present application provides a method for preparing lithium hydroxide from aluminum-based lithium concentrate, the method comprising:

[0034] S1, obtaining aluminum-based lithium concentrate slurry;

[0035] In some embodiments, the step of obtaining the aluminum-based lithium concentrate slurry comprises:

[0036] The aluminum-based lithium concentrate is mixed with water to obtain an aluminum-based lithium concentrate slurry; wherein the median particle size D50 of the aluminum-based lithium concentrate is 30 μm to 60 μm, and the solid content of the aluminum-based lithium concentrate slurry is 200 g / L to 600 g / L.

[0037] In the embodiment of the present application, the median particle size of the aluminum-based lithium concentrate can be 30μm to 60μm, because: the particle size of the aluminum-based lithium concentrate is negatively correlated with the alumina content in the aluminum-based lithium concentrate. The smaller the particle size of the aluminum-based lithium concentrate, the higher the alumina content, and the smaller the particle size, the higher the lithium content in the aluminum-based lithium concentrate, but the particle size becomes smaller after the subsequent leaching reaction, which makes filtering difficult; and the higher the particle size of the aluminum-based lithium concentrate, the lower the lithium content in the aluminum-based lithium concentrate, and the lower the concentration of lithium ions in the leachate, thereby affecting the subsequent lithium hydroxide concentration efficiency. Exemplarily, the median particle size of the above-mentioned aluminum-based lithium concentrate can be 30μm, 35μm, 40μm, 45μm, 50μm, 55μm, 60μm, etc. It should be noted that the solid content of the aluminum-based lithium concentrate slurry can be 200g / L to 600g / L. For example, the solid content of the aluminum-based lithium concentrate slurry can be 200g / L, 250g / L, 300g / L, 350g / L, 400g / L, 450g / L, 500g / L, 550g / L, 600g / L, etc. In addition, the Li2O content in the above aluminum-based lithium concentrate can be 0.2wt% to 2.0wt%.

[0038] S2, using an inorganic acid to leach the aluminum-based lithium concentrate slurry, and then performing solid-liquid separation to obtain a lithium-removed slag filter cake and a lithium nitrate solution;

[0039] In some embodiments, the inorganic acid comprises at least one of the following: sulfuric acid, nitric acid.

[0040] In some embodiments, the leaching process parameters include: temperature of 40°C to 80°C, and time of 0.5h to 3h.

[0041] In the embodiment of the present application, since the lithium in the aluminum-based lithium concentrate is in the form of Li2Al4(CO3)OH 12 · It exists in the form of 3H2O. Under normal conditions, it needs hydrothermal reaction at a higher temperature for leaching. Using inorganic acid to enhance leaching can achieve efficient lithium extraction at a lower temperature, reduce energy consumption, and also effectively remove CO3 in the solution. 2- , to prevent Li + With CO3 2- The reaction occurs and precipitates in advance. The leaching temperature can be 40°C to 80°C, and the leaching time can be 0.5h to 3h. The reason is to ensure the leaching effect of the aluminum-based lithium concentrate and achieve an aluminum-based lithium concentrate leaching rate of more than 98%. Exemplarily, the leaching temperature can be 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, etc., and the leaching time can be 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, etc.

[0042] In some embodiments, the amount of the inorganic acid used is 0.05% to 5% by weight of the aluminum-based lithium concentrate slurry.

[0043] In the embodiment of the present application, inorganic acid is used as a reagent for strengthening the leaching of aluminum-based lithium concentrate, which can achieve efficient leaching of lithium without introducing other secondary ions, thereby simplifying the impurity removal process. If the amount of inorganic acid is too low, it will lead to poor leaching effect and low leaching rate of aluminum-based lithium concentrate to a certain extent; if the amount of inorganic acid is too high, the impurity ions in the leached lithium-rich solution, including Ca 2+ Mg 2+ 、Al 3+ The content of the above inorganic acid increases, affecting the subsequent impurity removal effect. Exemplarily, the amount of the above inorganic acid is 0.05%, 0.07%, 0.09%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, etc. of the weight of the aluminum-based lithium concentrate slurry. The inorganic acid can be one or more of sulfuric acid and nitric acid. In the embodiment of the present application, concentrated sulfuric acid and concentrated nitric acid can be used.

[0044] In some embodiments, the median particle size D50 of the delithiation slag filter cake is 5 μm to 30 μm.

[0045] In an embodiment of the present application, after the lithium concentrate is leached by inorganic acid, the lithium-free slag filter cake is returned to prepare the lithium concentrate. If the median particle size of the lithium-free slag filter cake is too high, the lithium content in the prepared lithium concentrate may be low and the particle size may be too low, thereby affecting the filtering effect of the lithium concentrate and thus affecting the yield of the lithium hydroxide product. Exemplarily, the median particle size of the lithium-free slag filter cake can be 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 13 μm, 15 μm, 18 μm, 20 μm, 23 μm, 25 μm, 28 μm, 30 μm, etc.

[0046] S3, adjusting the pH of the lithium nitrate solution, and then performing fine filtration to obtain a fine filtrate;

[0047] In some embodiments, the target pH of the pH adjustment is 7-12.

[0048] In some embodiments, in the refined filtrate, the concentration of lithium ions is 0.1 g / L to 2 g / L, and the concentration of aluminum ions is ≤5 mg / L.

[0049] In the embodiment of the present application, the reason for adjusting the pH of the lithium salt solution to 7 to 12 is that by adjusting the pH of the solution, the aluminum ions in the solution can be effectively removed, while ensuring that the material properties meet the requirements of subsequent ion exchange purification and bipolar membrane operation. Exemplarily, the target pH of the above pH adjustment can be 7, 8, 9, 10, 11, 12, etc. Therefore, after adjusting the pH, the concentration of lithium ions in the fine filtrate can be 0.1g / L, 0.2g / L, 0.3g / L, 0.4g / L, 0.5g / L, 1g / L, 1.3g / L, 1.5g / L, 1.8g / L, 2g / L, etc., and the concentration of aluminum ions can be 5mg / L, 4mg / L, 3mg / L, 2mg / L, 1mg / L, etc.

[0050] S4, purifying the refined filtrate using an ion exchange resin to obtain a lithium salt pre-electrolyte;

[0051] In some embodiments, the Ca in the lithium salt pre-electrolyte is 2+ With Mg 2+ The mixed ion concentration is ≤2mg / L.

[0052] In the embodiment of the present application, the refined filtrate is purified by using an ion exchange resin to remove the Ca in the refined filtrate. 2+ Mg 2+ Impurity ions such as Ca2+ and Ca2+ can be removed to meet the purity requirements of lithium hydroxide products produced in the subsequent process. 2+ With Mg 2+ The mixed ion concentration can be 2 mg / L, 1.8 mg / L, 1.6 mg / L, 1.4 mg / L, etc.

[0053] S5. Perform bipolar membrane electrolysis on the lithium salt pre-electrolyte to obtain a lithium hydroxide solution and an inorganic acid.

[0054] In the embodiment of the present application, the process parameters of bipolar membrane electrolysis are current 5-10A; voltage 15-50V; bipolar membrane electrolysis time can be 10min-90min, which can increase the recovery rate of lithium and current efficiency, reduce energy consumption and improve the purity of the product solution. If the bipolar membrane electrolysis time is too long, the current efficiency is reduced, the concentration of lithium hydroxide in the solution no longer increases, and impurity ions are easily enriched; if the bipolar membrane electrolysis time is too short, the concentration of lithium hydroxide in the solution is low.

[0055] In some embodiments, the method further comprises:

[0056] S6. Evaporating and concentrating the lithium hydroxide solution to obtain a lithium hydroxide product; wherein the purity of the lithium hydroxide product is ≥99.5%.

[0057] In the embodiment of the present application, after bipolar membrane electrolysis treatment, the concentration of the cathode lithium hydroxide solution is 0.2wt% to 4.0wt%, which is beneficial to improving the evaporation crystallization efficiency; the anode inorganic acid is returned to the process after adjusting the concentration for leaching lithium concentrate, and the lithium hydroxide solution is evaporated, concentrated and crystallized to obtain a lithium hydroxide product.

[0058] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.

[0059] Example 1

[0060] A method for preparing lithium hydroxide from aluminum-based lithium concentrate, Figure 2 A schematic diagram of the actual process of preparing lithium hydroxide from an aluminum-based lithium concentrate provided in the embodiment of the present application; see Figure 2 , specifically including:

[0061] (1) Obtain aluminum-based lithium concentrate, add water to the aluminum-based lithium concentrate and stir to obtain a slurry.

[0062] The particle size D50 of the aluminum-based lithium concentrate is 60 μm; the Li2O content in the aluminum-based lithium concentrate is 0.2%, and the solid content of the aluminum-based lithium concentrate added is 200 g / L.

[0063] (2) adding nitric acid to the slurry, and after enhanced leaching, separating the solid and liquid to obtain a lithium-removed slag filter cake and a lithium nitrate solution.

[0064] The amount of nitric acid added was 0.05wt%, the reaction temperature was 40°C, the reaction time was 0.5h, and the leaching rate of the aluminum-based lithium concentrate was 99.5%.

[0065] (3) The de-lithium slag filter cake is recycled to prepare aluminum-based lithium concentrate.

[0066] After lithium concentrate is leached and delithiumized, the particle size D50 of the delithiumized slag filter cake is 30μm.

[0067] (4) The lithium nitrate solution is subjected to pH adjustment and fine filtration to obtain a fine filtrate.

[0068] The pH of lithium nitrate solution was adjusted to 7, and the refined filtrate Li + The concentration is 0.1g / L and the aluminum ion concentration is 1mg / L.

[0069] (5) Purifying the refined filtrate through ion exchange resin to remove impurities such as aluminum, calcium and magnesium in the solution to obtain a lithium nitrate pre-electrolyte.

[0070] Ca in the electrolyte pretreated with purified lithium nitrate 2+With Mg 2+ The mixed ion concentration is 0.5 mg / L.

[0071] (6) The lithium nitrate pre-electrolyte is treated by a bipolar membrane, and the lithium ions in the electrolyte combine with the decomposed hydroxide ions on the negative side of the bipolar membrane to form a lithium hydroxide solution, and the nitrate ions in the electrolyte combine with the decomposed hydrogen ions on the positive side of the bipolar membrane to form nitric acid.

[0072] The lithium nitrate pre-electrolyte was treated by a three-compartment bipolar membrane with a current of 5 A, a voltage of 15 V, and a bipolar membrane electrolysis time of 10 min.

[0073] (7) The lithium hydroxide solution is evaporated and crystallized to obtain a lithium hydroxide product, and the nitric acid is returned to the process for leaching lithium concentrate.

[0074] After bipolar membrane treatment, the concentration of the negative side lithium hydroxide solution is 0.2wt%. The lithium hydroxide solution is evaporated, concentrated and crystallized to obtain a lithium hydroxide product with a purity of 99.8%. The positive side nitric acid is returned to the process after the concentration is adjusted for leaching lithium concentrate.

[0075] Example 2

[0076] A method for preparing lithium hydroxide from aluminum-based lithium concentrate, specifically comprising:

[0077] (1) Obtain aluminum-based lithium concentrate, add water to the aluminum-based lithium concentrate and stir to obtain a slurry.

[0078] The particle size D50 of the aluminum-based lithium concentrate is 50 μm; the Li2O content in the aluminum-based lithium concentrate is 0.5%, and the solid content of the aluminum-based lithium concentrate added is 300 g / L.

[0079] (2) adding nitric acid to the slurry, and after enhanced leaching, separating the solid and liquid to obtain a lithium-removed slag filter cake and a lithium nitrate solution.

[0080] The amount of nitric acid added was 0.2wt%, the reaction temperature was 50°C, the reaction time was 1h, and the leaching rate of the aluminum-based lithium concentrate was 99.2%.

[0081] (3) The de-lithium slag filter cake is recycled to prepare aluminum-based lithium concentrate.

[0082] After lithium concentrate is leached and delithiumized, the particle size D50 of the delithiumized slag filter cake is 25 μm.

[0083] (4) The lithium nitrate solution is subjected to pH adjustment and fine filtration to obtain a fine filtrate.

[0084] The pH of lithium nitrate solution was adjusted to 8, and the refined filtrate Li + The concentration is 0.3g / L and the aluminum ion concentration is 2mg / L.

[0085] (5) Purifying the refined filtrate through ion exchange resin to remove impurities such as aluminum, calcium and magnesium in the solution to obtain a lithium nitrate pre-electrolyte.

[0086] Ca in the electrolyte pretreated with purified lithium nitrate 2+ With Mg 2+ The mixed ion concentration is 0.8 mg / L.

[0087] (6) The lithium nitrate pre-electrolyte is treated by a bipolar membrane, and the lithium ions in the electrolyte combine with the decomposed hydroxide ions on the negative side of the bipolar membrane to form a lithium hydroxide solution, and the nitrate ions in the electrolyte combine with the decomposed hydrogen ions on the positive side of the bipolar membrane to form nitric acid.

[0088] The lithium nitrate pre-electrolyte was treated by a three-compartment bipolar membrane with a current of 5 A, a voltage of 15 V, and a bipolar membrane electrolysis time of 20 min.

[0089] (7) The lithium hydroxide solution is evaporated and crystallized to obtain a lithium hydroxide product, and the nitric acid is returned to the process for leaching lithium concentrate.

[0090] After bipolar membrane treatment, the concentration of the negative side lithium hydroxide solution is 0.5wt%. The lithium hydroxide solution is evaporated, concentrated and crystallized to obtain a lithium hydroxide product with a purity of 99.7%. The positive side nitric acid is returned to the process after the concentration is adjusted for leaching lithium concentrate.

[0091] Example 3

[0092] A method for preparing lithium hydroxide from aluminum-based lithium concentrate, specifically comprising:

[0093] (1) Obtain aluminum-based lithium concentrate, add water to the aluminum-based lithium concentrate and stir to obtain a slurry.

[0094] The particle size D50 of the aluminum-based lithium concentrate is 45 μm; the Li2O content in the aluminum-based lithium concentrate is 1.2%, and the solid content of the aluminum-based lithium concentrate added is 400 g / L.

[0095] (2) adding nitric acid to the slurry, and after enhanced leaching, separating the solid and liquid to obtain a lithium-removed slag filter cake and a lithium nitrate solution.

[0096] The amount of nitric acid added was 1.0wt%, the reaction temperature was 60°C, the reaction time was 2h, and the leaching rate of the aluminum-based lithium concentrate was 99.0%.

[0097] (3) The de-lithium slag filter cake is recycled to prepare aluminum-based lithium concentrate.

[0098] After lithium concentrate is leached and delithiumized, the particle size D50 of the delithiumized slag filter cake is 20 μm.

[0099] (4) The lithium nitrate solution is subjected to pH adjustment and fine filtration to obtain a fine filtrate.

[0100] The pH of lithium nitrate solution was adjusted to 9, and the refined filtrate Li+ The concentration is 0.8g / L and the aluminum ion concentration is 2.5mg / L.

[0101] (5) Purifying the refined filtrate through ion exchange resin to remove impurities such as aluminum, calcium and magnesium in the solution to obtain a lithium nitrate pre-electrolyte.

[0102] Ca in the electrolyte pretreated with purified lithium nitrate 2+ With Mg 2+ The mixed ion concentration is 1 mg / L.

[0103] (6) The lithium nitrate pre-electrolyte is treated by a bipolar membrane, and the lithium ions in the electrolyte combine with the decomposed hydroxide ions on the negative side of the bipolar membrane to form a lithium hydroxide solution, and the nitrate ions in the electrolyte combine with the decomposed hydrogen ions on the positive side of the bipolar membrane to form nitric acid.

[0104] The lithium nitrate pre-electrolyte was treated by a three-compartment bipolar membrane with a current of 5 A, a voltage of 30 V, and a bipolar membrane electrolysis time of 20 min.

[0105] (7) The lithium hydroxide solution is evaporated and crystallized to obtain a lithium hydroxide product, and the nitric acid is returned to the process for leaching lithium concentrate.

[0106] After bipolar membrane treatment, the concentration of the negative side lithium hydroxide solution is 1wt%. The lithium hydroxide solution is evaporated, concentrated and crystallized to obtain a lithium hydroxide product with a purity of 99.6%. The positive side nitric acid is returned to the process after the concentration is adjusted for leaching lithium concentrate.

[0107] Example 4

[0108] A method for preparing lithium hydroxide from aluminum-based lithium concentrate, specifically comprising:

[0109] (1) Obtain aluminum-based lithium concentrate, add water to the aluminum-based lithium concentrate and stir to obtain a slurry.

[0110] The particle size D50 of the aluminum-based lithium concentrate is 40 μm; the Li2O content in the aluminum-based lithium concentrate is 1.5%, and the solid content of the aluminum-based lithium concentrate added is 500 g / L.

[0111] (2) adding nitric acid to the slurry, and after enhanced leaching, separating the solid and liquid to obtain a lithium-removed slag filter cake and a lithium nitrate solution.

[0112] The amount of nitric acid added was 3wt%, the reaction temperature was 60°C, the reaction time was 2.5h, and the leaching rate of aluminum-based lithium concentrate was 98.8%.

[0113] (3) The de-lithium slag filter cake is recycled to prepare aluminum-based lithium concentrate.

[0114] After lithium concentrate is leached and delithiumized, the particle size D50 of the delithiumized slag filter cake is 10 μm.

[0115] (4) The lithium nitrate solution is subjected to pH adjustment and fine filtration to obtain a fine filtrate.

[0116] The pH of lithium nitrate solution was adjusted to 10, and the refined filtrate Li + The concentration is 1.5g / L and the aluminum ion concentration is 3mg / L.

[0117] (5) Purifying the refined filtrate through ion exchange resin to remove impurities such as aluminum, calcium and magnesium in the solution to obtain a lithium nitrate pre-electrolyte.

[0118] Ca in the electrolyte pretreated with purified lithium nitrate 2+ With Mg 2+ The mixed ion concentration is 1.5 mg / L.

[0119] (6) The lithium nitrate pre-electrolyte is treated by a bipolar membrane, and the lithium ions in the electrolyte combine with the decomposed hydroxide ions on the negative side of the bipolar membrane to form a lithium hydroxide solution, and the nitrate ions in the electrolyte combine with the decomposed hydrogen ions on the positive side of the bipolar membrane to form nitric acid.

[0120] The lithium nitrate pre-electrolyte was treated by a three-compartment bipolar membrane with a current of 6 A, a voltage of 40 V, and a bipolar membrane electrolysis time of 40 min.

[0121] (7) The lithium hydroxide solution is evaporated and crystallized to obtain a lithium hydroxide product, and the nitric acid is returned to the process for leaching lithium concentrate.

[0122] After bipolar membrane treatment, the concentration of the negative side lithium hydroxide solution is 2wt%. The lithium hydroxide solution is evaporated, concentrated and crystallized to obtain a lithium hydroxide product with a purity of 99.6%. The positive side nitric acid is returned to the process after the concentration is adjusted for leaching lithium concentrate.

[0123] Example 5

[0124] A method for preparing lithium hydroxide from aluminum-based lithium concentrate, specifically comprising:

[0125] (1) Obtain aluminum-based lithium concentrate, add water to the aluminum-based lithium concentrate and stir to obtain a slurry.

[0126] The particle size D50 of the aluminum-based lithium concentrate is 30 μm; the Li2O content in the aluminum-based lithium concentrate is 2.0%, and the solid content of the aluminum-based lithium concentrate added is 600 g / L.

[0127] (2) adding nitric acid to the slurry, and after enhanced leaching, separating the solid and liquid to obtain a lithium-removed slag filter cake and a lithium nitrate solution.

[0128] The amount of nitric acid added was 5wt%, the reaction temperature was 80°C, the reaction time was 3h, and the leaching rate of aluminum-based lithium concentrate was 99.5%.

[0129] (3) The de-lithium slag filter cake is recycled to prepare aluminum-based lithium concentrate.

[0130] After lithium concentrate is leached and delithiumized, the particle size D50 of the delithiumized slag filter cake is 5 μm.

[0131] (4) The lithium nitrate solution is subjected to pH adjustment and fine filtration to obtain a fine filtrate.

[0132] The pH of lithium nitrate solution was adjusted to 12, and the refined filtrate Li + The concentration is 2g / L and the aluminum ion concentration is 5mg / L.

[0133] (5) Purifying the refined filtrate through ion exchange resin to remove impurities such as aluminum, calcium and magnesium in the solution to obtain a lithium nitrate pre-electrolyte.

[0134] Ca in the electrolyte pretreated with purified lithium nitrate 2+ With Mg 2+ The mixed ion concentration is 2mg / L.

[0135] (6) The lithium nitrate pre-electrolyte is treated by a bipolar membrane, and the lithium ions in the electrolyte combine with the decomposed hydroxide ions on the negative side of the bipolar membrane to form a lithium hydroxide solution, and the nitrate ions in the electrolyte combine with the decomposed hydrogen ions on the positive side of the bipolar membrane to form nitric acid.

[0136] The lithium nitrate pre-electrolyte was treated by a three-compartment bipolar membrane with a current of 10 A, a voltage of 50 V, and a bipolar membrane electrolysis time of 90 min;

[0137] (7) The lithium hydroxide solution is evaporated and crystallized to obtain a lithium hydroxide product, and the nitric acid is returned to the process for leaching lithium concentrate.

[0138] After bipolar membrane treatment, the concentration of the negative side lithium hydroxide solution is 4wt%. The lithium hydroxide solution is evaporated, concentrated and crystallized to obtain a lithium hydroxide product with a purity of 99.5%. The positive side nitric acid is returned to the process after the concentration is adjusted for leaching lithium concentrate.

[0139] Example 6

[0140] A method for preparing lithium hydroxide from aluminum-based lithium concentrate, specifically comprising:

[0141] (1) Obtain aluminum-based lithium concentrate, add water to the aluminum-based lithium concentrate and stir to obtain a slurry.

[0142] The particle size D50 of the aluminum-based lithium concentrate is 55 μm; the Li2O content in the aluminum-based lithium concentrate is 0.3%, and the solid content of the aluminum-based lithium concentrate added is 600 g / L.

[0143] (2) adding nitric acid to the slurry, and after enhanced leaching, separating the solid and liquid to obtain a lithium-removed slag filter cake and a lithium nitrate solution.

[0144] The amount of nitric acid added was 2 wt%, the reaction temperature was 70°C, the reaction time was 2 h, and the leaching rate of the aluminum-based lithium concentrate was 99.2%.

[0145] (3) The de-lithium slag filter cake is recycled to prepare aluminum-based lithium concentrate.

[0146] After lithium concentrate is leached and delithiumized, the particle size D50 of the delithiumized slag filter cake is 25 μm.

[0147] (4) The lithium nitrate solution is subjected to pH adjustment and fine filtration to obtain a fine filtrate.

[0148] The pH of lithium nitrate solution was adjusted to 8, and the refined filtrate Li + The concentration is 1.2g / L and the aluminum ion concentration is 2.5mg / L.

[0149] (5) Purifying the refined filtrate through an ion exchange resin to remove impurities such as aluminum, calcium, and magnesium in the solution to obtain a lithium nitrate pre-electrolyte.

[0150] Ca in the electrolyte pretreated with purified lithium nitrate 2+ With Mg 2+ The mixed ion concentration is 0.8 mg / L.

[0151] (6) The lithium nitrate pre-electrolyte is treated by a bipolar membrane, and the lithium ions in the electrolyte combine with the decomposed hydroxide ions on the negative side of the bipolar membrane to form a lithium hydroxide solution, and the nitrate ions in the electrolyte combine with the decomposed hydrogen ions on the positive side of the bipolar membrane to form nitric acid.

[0152] The lithium nitrate pre-electrolyte was treated by a three-compartment bipolar membrane with a current of 8 A, a voltage of 40 V, and a bipolar membrane electrolysis time of 40 min.

[0153] (7) The lithium hydroxide solution is evaporated and crystallized to obtain a lithium hydroxide product, and the nitric acid is returned to the process for leaching lithium concentrate.

[0154] After bipolar membrane treatment, the concentration of the negative side lithium hydroxide solution is 2wt%. The lithium hydroxide solution is evaporated, concentrated and crystallized to obtain a lithium hydroxide product with a purity of 99.6%. The positive side nitric acid is returned to the process after the concentration is adjusted for leaching lithium concentrate.

[0155] Example 7

[0156] A method for preparing lithium hydroxide from aluminum-based lithium concentrate, specifically comprising:

[0157] (1) Obtain aluminum-based lithium concentrate, add water to the aluminum-based lithium concentrate and stir to obtain a slurry.

[0158] The particle size D50 of the aluminum-based lithium concentrate is 30 μm; the Li2O content in the aluminum-based lithium concentrate is 2%, and the solid content of the aluminum-based lithium concentrate added is 200 g / L.

[0159] (2) adding nitric acid to the slurry, and after enhanced leaching, separating the solid and liquid to obtain a lithium-removed slag filter cake and a lithium nitrate solution.

[0160] The amount of nitric acid added was 0.05wt%, the reaction temperature was 45°C, the reaction time was 0.5h, and the leaching rate of the aluminum-based lithium concentrate was 98.5%.

[0161] (3) The de-lithium slag filter cake is recycled to prepare aluminum-based lithium concentrate.

[0162] After lithium concentrate is leached and delithiumized, the particle size D50 of the delithiumized slag filter cake is 5 μm.

[0163] (4) The lithium nitrate solution is subjected to pH adjustment and fine filtration to obtain a fine filtrate.

[0164] The pH of lithium nitrate solution was adjusted to 7, and the refined filtrate Li + The concentration is 1g / L and the aluminum ion concentration is 1mg / L.

[0165] (5) Purifying the refined filtrate through ion exchange resin to remove impurities such as aluminum, calcium and magnesium in the solution to obtain a lithium nitrate pre-electrolyte.

[0166] Ca in the electrolyte pretreated with purified lithium nitrate 2+ With Mg 2+ The mixed ion concentration is 1 mg / L.

[0167] (6) The lithium nitrate pre-electrolyte is treated by a bipolar membrane, and the lithium ions in the electrolyte combine with the decomposed hydroxide ions on the negative side of the bipolar membrane to form a lithium hydroxide solution, and the nitrate ions in the electrolyte combine with the decomposed hydrogen ions on the positive side of the bipolar membrane to form nitric acid.

[0168] The lithium nitrate pre-electrolyte was treated by a three-compartment bipolar membrane with a current of 5 A, a voltage of 40 V, and a bipolar membrane electrolysis time of 60 min.

[0169] (7) The lithium hydroxide solution is evaporated and crystallized to obtain a lithium hydroxide product, and the nitric acid is returned to the process for leaching lithium concentrate.

[0170] After bipolar membrane treatment, the concentration of the negative side lithium hydroxide solution is 2wt%. The lithium hydroxide solution is evaporated, concentrated and crystallized to obtain a lithium hydroxide product with a purity of 99.8%. The positive side nitric acid is returned to the process after the concentration is adjusted for leaching lithium concentrate.

[0171] Example 8

[0172] A method for preparing lithium hydroxide from aluminum-based lithium concentrate, specifically comprising:

[0173] (1) Obtain aluminum-based lithium concentrate, add water to the aluminum-based lithium concentrate and stir to obtain a slurry.

[0174] The particle size D50 of the aluminum-based lithium concentrate is 55 μm; the Li2O content in the aluminum-based lithium concentrate is 0.3%, and the solid content of the aluminum-based lithium concentrate added is 600 g / L.

[0175] (2) adding nitric acid to the slurry, and after enhanced leaching, separating the solid and liquid to obtain a lithium-removed slag filter cake and a lithium nitrate solution.

[0176] The amount of nitric acid added was 0.1wt%, the reaction temperature was 60°C, the reaction time was 3h, and the leaching rate of the aluminum-based lithium concentrate was 98.0%.

[0177] (3) The de-lithium slag filter cake is recycled to prepare aluminum-based lithium concentrate.

[0178] After lithium concentrate is leached and delithiumized, the particle size D50 of the delithiumized slag filter cake is 20 μm.

[0179] (4) The lithium nitrate solution is subjected to pH adjustment and fine filtration to obtain a fine filtrate.

[0180] The pH of lithium nitrate solution was adjusted to 10, and the refined filtrate Li + The concentration is 1.2g / L and the aluminum ion concentration is 1mg / L.

[0181] (5) Purifying the refined filtrate through ion exchange resin to remove impurities such as aluminum, calcium and magnesium in the solution to obtain a lithium nitrate pre-electrolyte.

[0182] Ca in the electrolyte pretreated with purified lithium nitrate 2+ With Mg 2+ The mixed ion concentration is 0.8 mg / L.

[0183] (6) The lithium nitrate pre-electrolyte is treated by a bipolar membrane, and the lithium ions in the electrolyte combine with the decomposed hydroxide ions on the negative side of the bipolar membrane to form a lithium hydroxide solution, and the nitrate ions in the electrolyte combine with the decomposed hydrogen ions on the positive side of the bipolar membrane to form nitric acid.

[0184] The lithium nitrate pre-electrolyte was treated by a three-compartment bipolar membrane with a current of 8 A, a voltage of 50 V, and a bipolar membrane electrolysis time of 40 min.

[0185] (7) The lithium hydroxide solution is evaporated and crystallized to obtain a lithium hydroxide product, and the nitric acid is returned to the process for leaching lithium concentrate.

[0186] After bipolar membrane treatment, the concentration of the negative side lithium hydroxide solution is 3wt%. The lithium hydroxide solution is evaporated, concentrated and crystallized to obtain a lithium hydroxide product with a purity of 99.7%. The positive side nitric acid is returned to the process after the concentration is adjusted for leaching lithium concentrate.

[0187] Example 9

[0188] A method for preparing lithium hydroxide from aluminum-based lithium concentrate, specifically comprising:

[0189] (1) Obtain aluminum-based lithium concentrate, add water to the aluminum-based lithium concentrate and stir to obtain a slurry.

[0190] The particle size D50 of the aluminum-based lithium concentrate is 40 μm; the Li2O content in the aluminum-based lithium concentrate is 1.5%, and the solid content of the aluminum-based lithium concentrate added is 500 g / L.

[0191] (2) Sulfuric acid is added to the slurry, and after enhanced leaching, solid-liquid separation is performed to obtain a lithium-removed slag filter cake and a lithium nitrate solution.

[0192] The amount of sulfuric acid added was 2.0wt%, the reaction temperature was 60°C, the reaction time was 2.5h, and the leaching rate of the aluminum-based lithium concentrate was 99.2%.

[0193] (3) The de-lithium slag filter cake is recycled to prepare aluminum-based lithium concentrate.

[0194] After lithium concentrate is leached and delithiumized, the particle size D50 of the delithiumized slag filter cake is 15 μm.

[0195] (4) The lithium sulfate solution is subjected to pH adjustment and fine filtration to obtain a fine filtrate.

[0196] The pH of lithium sulfate solution was adjusted to 7, and the refined filtrate Li + The concentration is 1.5g / L and the aluminum ion concentration is 3mg / L.

[0197] (5) Purifying the refined filtrate through ion exchange resin to remove impurities such as aluminum, calcium and magnesium in the solution to obtain a lithium sulfate pre-electrolyte.

[0198] Ca in the electrolyte pretreated with lithium sulfate after purification 2+ With Mg 2+ The mixed ion concentration is 1.5 mg / L.

[0199] (6) The lithium sulfate pre-electrolyte is treated by a bipolar membrane, and the lithium ions in the electrolyte combine with the decomposed hydroxide ions on the negative side of the bipolar membrane to form a lithium hydroxide solution, and the sulfate ions in the electrolyte combine with the decomposed hydrogen ions on the positive side of the bipolar membrane to form sulfuric acid.

[0200] The lithium sulfate pre-electrolyte was treated by a three-compartment bipolar membrane with a current of 6 A, a voltage of 40 V, and a bipolar membrane electrolysis time of 40 min.

[0201] (7) The lithium hydroxide solution is evaporated and crystallized to obtain a lithium hydroxide product, and the sulfuric acid is returned to the process for leaching lithium concentrate.

[0202] After bipolar membrane treatment, the concentration of the negative side lithium hydroxide solution is 2wt%. The lithium hydroxide solution is evaporated, concentrated and crystallized to obtain a lithium hydroxide product with a purity of 99.6%. The positive side sulfuric acid is returned to the process after the concentration is adjusted for leaching lithium concentrate.

[0203] Comparative Example 1

[0204] A method for preparing lithium hydroxide from aluminum-based lithium concentrate, Figure 2A schematic diagram of the actual process of preparing lithium hydroxide from an aluminum-based lithium concentrate provided in the embodiment of the present application; see Figure 2 , specifically including:

[0205] (1) Obtain aluminum-based lithium concentrate, add water to the aluminum-based lithium concentrate and stir to obtain a slurry.

[0206] The particle size D50 of the aluminum-based lithium concentrate is 60 μm; the Li2O content in the aluminum-based lithium concentrate is 0.2%, and the solid content of the aluminum-based lithium concentrate added is 200 g / L.

[0207] (2) After the slurry is heated and leached, solid-liquid separation is performed to obtain a lithium-removed slag filter cake and a lithium nitrate solution.

[0208] The process parameters of heating leaching are: temperature is 40°C, time is 0.5h, and the leaching rate of aluminum-based lithium concentrate is 60.0%.

[0209] (3) The de-lithium slag filter cake is recycled to prepare aluminum-based lithium concentrate.

[0210] After lithium concentrate is leached and delithiumized, the particle size D50 of the delithiumized slag filter cake is 30μm.

[0211] (4) The lithium nitrate solution is subjected to pH adjustment and fine filtration to obtain a fine filtrate.

[0212] The pH of lithium nitrate solution was adjusted to 7, and the refined filtrate Li + The concentration is 0.05g / L and the aluminum ion concentration is 1mg / L.

[0213] (5) Purifying the refined filtrate through ion exchange resin to remove impurities such as aluminum, calcium and magnesium in the solution to obtain a lithium nitrate pre-electrolyte.

[0214] Ca in the electrolyte pretreated with purified lithium nitrate 2+ With Mg 2+ The mixed ion concentration is 0.5 mg / L.

[0215] (6) The lithium nitrate pre-electrolyte is treated by a bipolar membrane, and the lithium ions in the electrolyte combine with the decomposed hydroxide ions on the negative side of the bipolar membrane to form a lithium hydroxide solution, and the nitrate ions in the electrolyte combine with the decomposed hydrogen ions on the positive side of the bipolar membrane to form nitric acid.

[0216] The lithium nitrate pre-electrolyte was treated by a three-compartment bipolar membrane with a current of 5 A, a voltage of 15 V, and a bipolar membrane electrolysis time of 10 min.

[0217] (7) The lithium hydroxide solution is evaporated and crystallized to obtain a lithium hydroxide product, and the nitric acid is returned to the process for leaching lithium concentrate.

[0218] After bipolar membrane treatment, the concentration of the negative side lithium hydroxide solution is 0.1wt%. The lithium hydroxide solution is evaporated, concentrated and crystallized to obtain a lithium hydroxide product with a purity of 99.0%. The positive side nitric acid is returned to the process after the concentration is adjusted for leaching lithium concentrate.

[0219] Comparative Example 2

[0220] A method for preparing lithium hydroxide from aluminum-based lithium concentrate, specifically comprising:

[0221] (1) Obtain aluminum-based lithium concentrate, add water to the aluminum-based lithium concentrate and stir to obtain a slurry.

[0222] The particle size D50 of the aluminum-based lithium concentrate is 60 μm; the Li2O content in the aluminum-based lithium concentrate is 0.2%, and the solid content of the aluminum-based lithium concentrate added is 200 g / L.

[0223] (2) adding nitric acid to the slurry, and after enhanced leaching, separating the solid and liquid to obtain a lithium-removed slag filter cake and a lithium nitrate solution.

[0224] The amount of nitric acid added was 8 wt %, the reaction temperature was 40° C., the reaction time was 0.5 h, and the leaching rate of the aluminum-based lithium concentrate was 99.6%.

[0225] (3) The de-lithium slag filter cake is recycled to prepare aluminum-based lithium concentrate.

[0226] After lithium concentrate is leached and delithiumized, the particle size D50 of the delithiumized slag filter cake is 30μm.

[0227] (4) The lithium nitrate solution is subjected to pH adjustment and fine filtration to obtain a fine filtrate.

[0228] The pH of lithium nitrate solution was adjusted to 7, and the refined filtrate Li + The concentration is 0.1g / L and the aluminum ion concentration is 1mg / L.

[0229] (5) Purifying the refined filtrate through ion exchange resin to remove impurities such as aluminum, calcium and magnesium in the solution to obtain a lithium nitrate pre-electrolyte.

[0230] Ca in the electrolyte pretreated with purified lithium nitrate 2+ With Mg 2+ The mixed ion concentration is 5mg / L.

[0231] (6) The lithium nitrate pre-electrolyte is treated by a bipolar membrane, and the lithium ions in the electrolyte combine with the decomposed hydroxide ions on the negative side of the bipolar membrane to form a lithium hydroxide solution, and the nitrate ions in the electrolyte combine with the decomposed hydrogen ions on the positive side of the bipolar membrane to form nitric acid.

[0232] The lithium nitrate pre-electrolyte was treated by a three-compartment bipolar membrane with a current of 5 A, a voltage of 15 V, and a bipolar membrane electrolysis time of 10 min.

[0233] (7) The lithium hydroxide solution is evaporated and crystallized to obtain a lithium hydroxide product, and the nitric acid is returned to the process for leaching lithium concentrate.

[0234] After the bipolar membrane treatment, the concentration of the negative side lithium hydroxide solution is 0.2wt%, and the lithium hydroxide solution is evaporated, concentrated and crystallized to obtain a lithium hydroxide product with a purity of 96.0%. The positive side nitric acid is returned to the process after the concentration is adjusted for leaching lithium concentrate. The technical effect of the method for preparing lithium hydroxide from an aluminum-based lithium concentrate provided in Examples 1 to 8 and Comparative Examples 1 to 2 is evaluated, and the results are shown in Table 1 for the purity and lithium extraction rate of the lithium hydroxide product.

[0235] Table 1 Purity and lithium extraction rate of lithium hydroxide products

[0236] Serial number Lithium extraction rate % Purity of lithium hydroxide product % Example 1 99.5 99.8 Example 2 99.2 99.7 Example 3 99.0 99.6 Example 4 98.8 99.6 Example 5 99.5 99.5 Example 6 99.2 99.6 Example 7 98.5 99.8 Example 8 98.0 99.7 Example 9 99.2 99.6 Comparative Example 1 60.0 99.0 Comparative Example 2 99.6 96.0

[0237] As can be seen from Table 1, the lithium extraction rate of the preparation method of Examples 1-9 of the present application is ≥98%, and the purity of the lithium hydroxide product is ≥99.5%, which is significantly better than the lithium extraction rate and the purity of the aluminum hydroxide product of Comparative Examples 1-2. Specifically, in Comparative Example 1, when no inorganic acid is added, the lithium extraction rate is significantly reduced, and the lithium content in the refined filtrate is relatively low; in Comparative Example 2, when the amount of inorganic acid added is too high, although the lithium extraction rate is high, the impurity ions (Ca 2+ With Mg 2+ The mixed ion concentration) increased, resulting in a decrease in the purity of the final lithium hydroxide product.

[0238] One or more technical solutions in the embodiments of the present application also have at least the following technical effects or advantages:

[0239] (1) Inorganic acid treatment of aluminum-based lithium concentrate with Li2Al4(CO3)OH 12 · Lithium in the form of 3H2O can be leached to achieve efficient extraction of lithium from aluminum-based lithium concentrate. The leaching rate of aluminum-based lithium concentrate can reach more than 98%. At the same time, CO3 can also be effectively removed from aluminum-based lithium concentrate slurry. 2- , thereby preventing Li in aluminum-based lithium concentrate slurry + With CO3 2- The reaction occurs and precipitates in advance, and the introduction of other impurity ions is avoided, simplifying the impurity removal process;

[0240] (2) After solid-liquid separation, pH adjustment and fine filtration, the impurity ions in the leached slurry can be removed to a large extent, so that a pure fine filtrate containing lithium ions can be obtained; the lithium salt pre-electrolyte is subjected to bipolar membrane electrolysis, and the products are lithium hydroxide solution and inorganic acid. The lithium hydroxide solution can be evaporated and crystallized to obtain a lithium hydroxide product with a purity of ≥99.5%. The inorganic acid can be returned to the process after adjusting the concentration for leaching lithium concentrate, thereby realizing efficient and full-quantity utilization of aluminum-based lithium concentrate;

[0241] (3) Inorganic acid is combined with low temperature conditions to leach lithium, and the amount of inorganic acid added is small, achieving a high lithium extraction rate;

[0242] (4) The method for preparing lithium hydroxide from aluminum-based lithium concentrate provided in the embodiment of the present application provides a new technical route for the application of aluminum-based lithium concentrate and solves the technical problems of low lithium recovery rate in aluminum-based lithium concentrate and inability to recycle the recovered products;

[0243] (5) The embodiments of the present application overcome the defects of the prior art in preparing lithium hydroxide products from lithium-containing raw materials, such as low leaching rate, high energy consumption, long process and complex purification process.

[0244] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A method for preparing lithium hydroxide from aluminum-based lithium concentrate, characterized in that: The method comprises: Obtaining aluminum-based lithium concentrate slurry; The aluminum-based lithium concentrate slurry is leached using an inorganic acid, and then solid-liquid separation is performed to obtain a lithium-removed slag filter cake and a lithium salt solution; The lithium salt solution is subjected to pH adjustment and then fine filtration to obtain a fine filtrate; Purifying the refined filtrate using an ion exchange resin to obtain a lithium salt pre-electrolyte; The lithium salt pre-electrolyte is subjected to bipolar membrane electrolysis to obtain a lithium hydroxide solution and an inorganic acid.

2. The method according to claim 1, characterized in that The method for obtaining the aluminum-based lithium concentrate slurry comprises: The aluminum-based lithium concentrate is mixed with water to obtain an aluminum-based lithium concentrate slurry; wherein the median particle size of the aluminum-based lithium concentrate is 30 μm to 60 μm, and the solid content of the aluminum-based lithium concentrate slurry is 200 g / L to 600 g / L.

3. The method according to claim 1, characterized in that The inorganic acid includes at least one of the following: sulfuric acid and nitric acid.

4. The method according to claim 1 or 3, characterized in that: The dosage of the inorganic acid is 0.05% to 5% of the weight of the aluminum-based lithium concentrate slurry.

5. The method according to claim 1, characterized in that The leaching process parameters include: temperature of 40° C. to 80° C. and time of 0.5 h to 3 h.

6. The method according to claim 1, characterized in that The target pH of the pH adjustment is 7-12.

7. The method according to claim 1 or 6, characterized in that: In the refined filtrate, the concentration of lithium ions is 0.1 g / L to 2 g / L, and the concentration of aluminum ions is ≤5 mg / L.

8. The method according to claim 1, characterized in that The Ca in the lithium salt pre-electrolyte 2+ With Mg 2+ The mixed ion concentration is ≤2mg / L.

9. The method according to claim 1, characterized in that: The median particle size of the lithium-removing slag filter cake is 5 μm to 30 μm.

10. The method according to claim 1, characterized in that The method further comprises: The lithium hydroxide solution is evaporated and concentrated to obtain a lithium hydroxide product; wherein the purity of the lithium hydroxide product is ≥99.5%.