Spinel type high-entropy oxide photoelectric catalytic material and application
Preparation of spinel-type high-entropy oxide CuM2O4 through high-temperature solid-phase reactions solves the problem of insufficient material performance in the prior art, achieves efficient photoelectro-catalytic decomposition of water and pollutant degradation effects, and improves solar energy utilization efficiency.
Patent Information
- Application Number
- CN202410996437.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
AI Technical Summary
The lack of research and application of spinel-type high-entropy oxide photoelectro-catalytic materials in the prior art has led to insufficient material performance in the fields of photoelectro-catalytic decomposition of water and other fields, and the inability to effectively utilize solar energy.
The spinel-type high-entropy oxide CuM2O4 is prepared through high-temperature solid phase reaction, and the radiation heating sintering method is used to ensure that the material has a tetraquartile core cell and an I41/amd space group structure, including metal elements such as Al and Ga, and improve its photoelectric catalysis. Activity and stability.
The high photoelectrocatalytic activity and stability of spinel-type high-entropy oxide photoelectrocatalytic materials are achieved, which significantly enhances the catalytic activity and selectivity of the catalyst and improves the utilization efficiency of solar energy.
Smart Images

Figure CN118932373A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of photoelectrocatalytic materials, and in particular relates to a spinel-type high-entropy oxide photoelectrocatalytic material and an application thereof. Background Art
[0002] Solar energy is a dispersed, inexhaustible natural resource. Researchers have found that the amount of solar energy radiating to the Earth’s surface (1.3×10 5 TW) is far higher than the current total global energy consumption. Converting solar energy into stable chemical energy is considered one of the most promising strategies to solve energy and environmental problems. Photoelectrocatalytic water splitting technology is a recognized green technology for converting solar energy into stable chemical energy. Since the solar spectrum is mainly composed of visible light (≥45%), improving the utilization rate of visible light by photoelectrodes is one of the prerequisites for efficient use of solar energy.
[0003] Spinel compounds have rich compositions and structures, and flexible and adjustable physical and chemical properties, making ferroxite-type oxides one of the hot materials in the fields of photovoltaics, photocatalysis, and photoelectrocatalysis. Spinel-type high-entropy oxides have high entropy values, low Gibbs free energy, and abundant reaction active sites. They exhibit excellent performance in the fields of optics, electricity, and energy, and have broad application prospects. There are currently no reports on spinel-type high-entropy oxide photoelectrocatalytic materials. The present invention prepares a spinel-type high-entropy oxide photoelectrocatalytic material by high-temperature solid-phase reaction, and applies the material to the photoelectrocatalytic decomposition of water to produce hydrogen. Summary of the invention
[0004] In view of the above-mentioned shortcomings of the prior art, the present invention provides a spinel-type high-entropy oxide photoelectrocatalytic material and application thereof.
[0005] To achieve the above object, the technical solution adopted by the present invention is:
[0006] A spinel-type high-entropy oxide photoelectrocatalytic material has a chemical formula of CuM2O4, a spinel structure, a tetragonal body-centered unit cell, belongs to the tetragonal crystal system, and has a space group of I41 / amd; M is 5 to 8 of the elements Al, Ga, V, Cr, Mn, Fe, Co, and Ni, and the molar percentage of each M element is 10 to 20%; wherein M contains at least one of Al and Ga.
[0007] The method for preparing the spinel-type high entropy oxide photoelectrocatalytic material comprises: mixing copper oxide and an oxide of metal M and sintering the mixture to obtain the spinel-type high entropy oxide photoelectrocatalytic material.
[0008] As a preferred embodiment of the present invention, the spinel-type high entropy oxide photoelectrocatalytic material is a single spinel structure.
[0009] As a preferred embodiment of the present invention, the heating method used for sintering is radiation heating.
[0010] As a preferred embodiment of the present invention, the sintering temperature is 900-1200° C., the sintering time is 4-30 hours, and the atmosphere is oxygen or air.
[0011] As a preferred embodiment of the present invention, the sintering times are 3 or more.
[0012] The present invention also claims to protect the application of the spinel-type high entropy oxide photoelectrocatalytic material in photocatalytic water splitting to produce hydrogen.
[0013] The present invention also claims to protect the application of the spinel-type high entropy oxide photoelectrocatalytic material in the removal of organic pollutants or heavy metals.
[0014] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention obtains a spinel-type high entropy oxide photoelectrocatalytic material CuM2O4 with a tetragonal body-centered unit cell and a space group of I41 / amd through reasonable element design, and the CuM2O4 has high photoelectrocatalytic activity and stability. In addition, the synergistic effect between the metal ions of the spinel-type high entropy oxide species can effectively improve the carrier separation rate, optical properties, electronic structure and energy band structure of the spinel-type photoelectrocatalytic material, and can significantly enhance the catalytic activity of the catalyst. And the abundant metal elements in CuM2O4 provide abundant reaction active sites for the photoelectrocatalytic reaction, thereby improving the catalytic reaction activity and selectivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is the X-ray diffraction pattern of the Cu(GaCrMnFeCoNi)2O4 spinel high entropy oxide photoelectrocatalytic material prepared in Example 1.
[0016] Figure 2 This is the UV-visible diffuse reflection absorption spectrum of the Cu(GaCrMnFeCoNi)2O4 spinel high entropy oxide photoelectrocatalytic material prepared in Example 1.
[0017] Figure 3 This is the time-current curve of the Cu(GaCrMnFeCoNi)2O4 spinel high entropy oxide photoelectrocatalytic material prepared in Example 1.
[0018] Figure 4 This is the photocatalytic water decomposition and hydrogen production performance diagram of the Cu(GaCrMnFeCoNi)2O4 spinel high entropy oxide photoelectrocatalytic material prepared in Example 1.
[0019] Figure 5This is the performance diagram of the photocatalytic degradation of methylene blue pollutant by the Cu(GaCrMnFeCoNi)2O4 spinel high entropy oxide photoelectrocatalytic material prepared in Example 1.
[0020] Figure 6 X-ray crystal diffraction pattern of the Cu(GaCrMnFeCoNi)2O4 spinel high entropy oxide photoelectrocatalytic material prepared in Example 1 before and after photocatalytic degradation of methylene blue, wherein As prepared is the XRD pattern before photocatalytic degradation of methylene blue, and After PEC test is the XRD pattern after photocatalytic degradation of methylene blue.
[0021] Figure 7 This is the X-ray diffraction pattern of the Cu(AlCrMnFeCoNi)2O4 spinel high entropy oxide photoelectrocatalytic material prepared in Example 2.
[0022] Figure 8 This is the UV-visible diffuse reflection absorption spectrum of the Cu(AlCrMnFeCoNi)2O4 spinel high entropy oxide photoelectrocatalytic material prepared in Example 2.
[0023] Fig. 9 This is the time-current curve of the Cu(AlCrMnFeCoNi)2O4 spinel high entropy oxide photoelectrocatalytic material prepared in Example 2.
[0024] Fig.10 The photocatalytic water decomposition hydrogen production rate and cyclic stability diagram of the Cu(AlCrMnFeCoNi)2O4 spinel high entropy oxide photoelectrocatalytic material prepared in Example 2.
[0025] Fig.11 This is the performance diagram of the photocatalytic degradation of methyl orange pollutants by the Cu(AlCrMnFeCoNi)2O4 spinel high entropy oxide photoelectrocatalytic material prepared in Example 2.
[0026] Fig.12 This is the X-ray diffraction pattern of the Cu(GaCrMnFeCo)2O4 spinel high entropy oxide photoelectrocatalytic material prepared in Example 3.
[0027] Fig.13 This is the UV-visible diffuse reflection absorption spectrum of the Cu(GaCrMnFeCo)2O4 spinel high entropy oxide photoelectrocatalytic material prepared in Example 3.
[0028] Fig.14 This is the LSV curve of the Cu(GaCrMnFeCo)2O4 spinel high entropy oxide photoelectrocatalytic material prepared in Example 3.
[0029] Fig.15This is the time-current curve of the Cu(GaCrMnFeCo)2O4 spinel high entropy oxide photoelectrocatalytic material prepared in Example 3.
[0030] Fig.16 This is the photocatalytic water decomposition and hydrogen production performance diagram of the Cu(GaCrMnFeCo)2O4 spinel high entropy oxide photoelectrocatalytic material prepared in Example 3.
[0031] Fig.17 This is the performance diagram of the photocatalytic degradation of tetracycline hydrochloride pollutant by the Cu(GaCrMnFeCo)2O4 spinel high entropy oxide photoelectrocatalytic material prepared in Example 3.
[0032] Fig.18 This is the time-current curve of the Cu(AlCrMnFeCo)2O4 spinel high entropy oxide photoelectrocatalytic material prepared in Example 4.
[0033] Fig.19 This is the photocatalytic water decomposition and hydrogen production performance diagram of the Cu(AlCrMnFeCo)2O4 spinel high entropy oxide photoelectrocatalytic material prepared in Example 4.
[0034] Fig. 20 The photocatalytic reduction of Cr by the Cu(AlCrMnFeCo)2O4 spinel high entropy oxide photoelectrocatalytic material prepared in Example 4 6+ Performance graph.
[0035] Fig.21 This is a graph showing the degradation rate of methylene blue pollutants photocatalytically degraded by the Cu(AlGaVCrMnFeCo)2O4 spinel high entropy oxide photoelectrocatalytic material prepared in Example 5.
[0036] Fig. 22 The photocatalytic water decomposition hydrogen production rate and cyclic stability diagram of the Cu(AlGaVCrMnFeCo)2O4 spinel high entropy oxide photoelectrocatalytic material prepared in Example 5.
[0037] Fig.23 This is the photocatalytic water decomposition and hydrogen production performance diagram of the Cu(AlGaCrMnFeCoNi)2O4 spinel high entropy oxide photoelectrocatalytic material prepared in Example 6.
[0038] Fig.24 This is the performance diagram of the photocatalytic degradation of methylene blue pollutants by the Cu(AlGaCrMnFeCoNi)2O4 spinel high entropy oxide photoelectrocatalytic material prepared in Example 6.
[0039] Fig.25This is the LSV curve of the Cu(AlGaVCrMnFeCoNi)2O4 spinel high entropy oxide photoelectrocatalytic material prepared in Example 7.
[0040] Fig.26 This is the time-current curve of the Cu(AlGaVCrMnFeCoNi)2O4 spinel high entropy oxide photoelectrocatalytic material prepared in Example 7.
[0041] Fig. 27 This is the performance diagram of the photocatalytic degradation of tetracycline hydrochloride pollutant by the Cu(AlGaVCrMnFeCoNi)2O4 spinel high entropy oxide photoelectrocatalytic material prepared in Example 7.
[0042] Fig.28 This is the time-current curve of the Cu(GaMnFe)2O4 spinel medium-entropy oxide photoelectrocatalytic material prepared in Comparative Example 1.
[0043] Fig.29 This is the performance diagram of the photocatalytic degradation of tetracycline hydrochloride pollutant by the Cu(GaMnFe)2O4 spinel medium entropy oxide photoelectrocatalytic material prepared in Comparative Example 1.
[0044] Fig.30 This is the photocatalytic water decomposition and hydrogen production performance diagram of the Cu(GaMnFe)2O4 spinel medium-entropy oxide photoelectrocatalytic material prepared in Comparative Example 1.
[0045] Fig.31 This is the time-current curve of the CuFe2O4 spinel low-entropy oxide photoelectrocatalytic material prepared in Comparative Example 2.
[0046] Fig.32 This is the performance diagram of the photocatalytic degradation of tetracycline hydrochloride pollutant by the CuFe2O4 spinel low entropy oxide photoelectrocatalytic material prepared in Comparative Example 2.
[0047] Fig.33 This is the photocatalytic water decomposition and hydrogen production performance diagram of the CuFe2O4 spinel low-entropy oxide photoelectrocatalytic material prepared in Comparative Example 2.
[0048] Fig.34 This is the X-ray diffraction pattern of the Cu(GaCrMnFeCoNi)2O4 spinel high entropy oxide photoelectrocatalytic material prepared in Comparative Example 3.
[0049] Fig.35 This is the X-ray diffraction pattern of the Cu(VCrMnFeNi)2O4 high entropy oxide photoelectrocatalytic material prepared in Comparative Example 4.
[0050] Fig.36This is the X-ray diffraction pattern of the Cu(GaCrMnFeCoBi)2O4 high entropy oxide photoelectrocatalytic material prepared in Comparative Example 5. DETAILED DESCRIPTION
[0051] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.
[0052] Example 1
[0053] A method for preparing a Cu(GaCrMnFeCoNi)2O4 spinel high entropy oxide photoelectrocatalytic material, the specific steps are as follows:
[0054] (1) Accurately weigh 0.7955 g CuO, 0.313 g Ga2O3, 0.2538 g Cr2O3, 0.2904 g MnO2, 0.2667 g Fe2O3, 0.277 g Co2O3, and 0.2495 g NiO metal oxide powders, transfer them to an agate mortar, add a small amount of anhydrous ethanol, and grind for 2 h to obtain powder A.
[0055] (2) Powder A is placed in a mold and pressed into a circular ceramic piece B by cold isostatic pressing.
[0056] (3) Ceramic piece B was placed in a corundum crucible and transferred to a tube furnace. The temperature was raised to 1000°C at a rate of 5°C / min in an air atmosphere and kept at this temperature for 10 h to obtain ceramic sample C.
[0057] (4) After grinding the ceramic sample C, repeat step (3) twice to obtain a high-purity spinel high-entropy oxide photoelectrocatalytic material.
[0058] Depend on Figure 1 It can be seen that the characteristic diffraction peaks of Cu(GaCrMnFeCoNi)2O4 prepared in Example 1 completely correspond to the standard PDF card of spinel oxides with tetragonal body-centered unit cell and I41 / amd space group, indicating that spinel high entropy oxides have been successfully prepared. Figure 2 It can be seen that the light absorption range of Cu(GaCrMnFeCoNi)2O4 covers the ultraviolet light region, visible light and part of near-infrared light, and can absorb and utilize sunlight to the maximum extent.
[0059] Depend on Figure 3 It can be seen that the photocurrent density generated by the Cu(GaCrMnFeCoNi)2O4 photoelectrode prepared in Example 1 under the irradiation of visible light emitted by a 300W xenon lamp is about 140μA / cm 2 , has a high catalytic activity. Figure 4It can be seen that when methanol is used as a hole sacrificial agent, 0.01 g of the photocatalyst decomposes water at a wavelength of 400 nm to produce a large amount of hydrogen, which produces a strong hydrogen signal in the gas chromatograph.
[0060] Depend on Figure 5 It can be seen that the Cu(GaCrMnFeCoNi)2O4 photoelectrocatalyst prepared in Example 1 exhibits excellent photocatalytic degradation of pollutants under visible light irradiation from a 300W xenon lamp. 50 mg of the catalyst was dispersed in 100 mL of methylene blue solution and placed in a dark box after ultrasonic dispersion. After 20 minutes of dark reaction to reach adsorption equilibrium, the xenon lamp was turned on and 4 mL of the stock solution was taken every 10 minutes. After two centrifugations, the supernatant was placed in a cuvette and the absorbance of the liquid was tested under an ultraviolet spectrophotometer. It can be found that the degradation rate of methylene blue by Cu(GaCrMnFeCoNi)2O4 can reach 98.2% within 60 minutes. After the test is completed, the catalyst sample after reaction is filtered by a vacuum filter and dried, and the XRD of the sample after reaction is tested. As Figure 6 It can be found that the catalyst has excellent stability. After the catalytic reaction, the high-entropy phase of Cu(GaCrMnFeCoNi)2O4 hardly changes, and no X-ray diffraction peaks corresponding to impurities (such as CuO, Fe2O3) are detected.
[0061] Example 2
[0062] A method for preparing a Cu(AlCrMnFeCoNi)2O4 spinel high entropy oxide photoelectrocatalytic material, the specific steps are as follows:
[0063] (1) Accurately weigh 0.7955 g CuO, 0.1703 g Al2O3, 0.2538 g Cr2O3, 0.2904 g MnO2, 0.2667 g Fe2O3, 0.277 g Co2O3, and 0.2495 g NiO metal oxide powders, transfer them to an agate mortar, add a small amount of anhydrous ethanol, and grind for 2 h to obtain powder A.
[0064] (2) Powder A is placed in a mold and pressed into a circular ceramic piece B by cold isostatic pressing.
[0065] (3) Ceramic piece B was placed in a corundum crucible and transferred to a tube furnace. The temperature was raised to 1100°C at a rate of 5°C / min in an air atmosphere and kept at this temperature for 12 h to obtain ceramic sample C.
[0066] (4) After grinding the ceramic sample C, repeat step (3) twice to obtain a high-purity spinel high-entropy oxide photoelectrocatalytic material.
[0067] Depend on Figure 7It can be seen that the characteristic diffraction peaks of Cu(AlCrMnFeCoNi)2O4 prepared in Example 2 completely correspond to the standard PDF card of spinel oxides with tetragonal body-centered unit cell and I41 / amd space group, indicating that spinel high entropy oxides have been successfully prepared. Figure 8 It can be seen that the light absorption range of Cu(AlCrMnFeCoNi)2O4 covers the ultraviolet light region, visible light and part of near-infrared light, and can absorb and utilize sunlight to the maximum extent.
[0068] Depend on Fig. 9 It can be seen that the photocurrent density generated by the Cu(AlCrMnFeCoNi)2O4 photoelectrode under the irradiation of visible light emitted by a 300W xenon lamp is about 120μA / cm 2 , showing excellent photoelectrocatalytic performance in decomposing water to produce hydrogen. Fig.10 It can be seen that when methanol is used as a hole sacrificial agent, the photocatalytic decomposition of water and hydrogen production rate of 0.01gCu(AlCrMnFeCoNi)2O4 photocatalyst under visible light irradiation is about 580μmol / g / h, showing a high performance of decomposition of water and hydrogen production. And after 5 cycles, the decomposition of water and hydrogen production rate is still maintained at about 550μmol / g / h, with excellent catalytic stability, which can adapt to long-term catalytic reaction tests.
[0069] Depend on Fig.11 It can be seen that the Cu(AlCrMnFeCoNi)2O4 photocatalyst exhibits excellent photocatalytic degradation of pollutants under the irradiation of visible light emitted by a 300W xenon lamp. 20mg of the catalyst was dispersed in 100mL of methyl orange solution and placed in a dark box after ultrasonic dispersion. After 30 minutes of dark reaction to reach adsorption equilibrium, the xenon lamp was turned on and 4mL of the stock solution was taken every 15 minutes. After two centrifugations, the supernatant was placed in a cuvette and the absorbance of the liquid was tested under a UV spectrophotometer. It can be found that the degradation rate of methyl orange by Cu(AlCrMnFeCoNi)2O4 can reach 98.8% within 60 minutes.
[0070] Example 3
[0071] A method for preparing a Cu(GaCrMnFeCo)2O4 spinel high entropy oxide photoelectrocatalytic material, the specific steps are as follows:
[0072] (1) Accurately weigh 0.7955 g CuO, 0.3749 g Ga2O3, 0.3040 g Cr2O3, 0.3477 g MnO2, 0.3194 g Fe2O3, and 0.3317 g Co2O3 metal oxide powders, transfer them to an agate mortar, add a small amount of anhydrous ethanol, and grind for 0.5 h to obtain powder A.
[0073] (2) Powder A is placed in a mold and pressed into a circular ceramic piece B by cold isostatic pressing.
[0074] (3) Ceramic piece B was placed in a corundum crucible and transferred to a tube furnace. The temperature was raised to 900°C at a rate of 5°C / min in an air atmosphere and kept at that temperature for 6 h to obtain ceramic sample C.
[0075] (4) After grinding the ceramic sample C, repeat step (3) twice to obtain a high-purity spinel high-entropy oxide photoelectrocatalytic material.
[0076] Depend on Fig.12 It can be seen that the characteristic diffraction peaks of Cu(GaCrMnFeCo)2O4 completely correspond to the standard PDF card of spinel oxides with tetragonal body-centered unit cell and I41 / amd space group, indicating that spinel high entropy oxides have been successfully prepared. Fig.13 It can be seen that the light absorption range of Cu(GaCrMnFeCo)2O4 covers the ultraviolet light region, visible light and part of near-infrared light, and it can absorb and utilize sunlight very well.
[0077] Depend on Fig.14 It can be seen that under visible light irradiation, -0.4V Ag / AgCl Under voltage, the photocurrent density of Cu(GaCrMnFeCo)2O4 can reach up to 2.4mA / cm 2 , which has a high performance of photoelectrocatalytic water decomposition and hydrogen production.
[0078] Depend on Fig.15 It can be seen that under visible light irradiation, at 0V Ag / AgCl Under voltage, the photocurrent density of Cu(GaCrMnFeCo)2O4 in three cycle tests was 89.0μA / cm 2 , 85.4μA / cm 2 and 83.1μA / cm 2 After three cycles of testing, the photoelectrocatalytic activity was still maintained at about 93%, indicating that the Cu(GaCrMnFeCo)2O4 spinel high entropy oxide has good catalytic stability.
[0079] The Cu(GaCrMnFeCo)2O4 photocatalyst prepared in Example 3 exhibits excellent photocatalytic performance in decomposing water to produce hydrogen under irradiation of a 300W xenon lamp. Fig.16 It can be seen that when methanol is used as a hole sacrificial agent, 0.01 g of the photocatalyst decomposes water at a wavelength of 400 nm to produce a large amount of hydrogen, which produces a strong hydrogen signal in the gas chromatograph.
[0080] Depend on Fig.17It can be seen that the Cu(GaCrMnFeCo)2O4 photoelectrocatalyst prepared in this embodiment exhibits excellent photocatalytic degradation of pollutants under the irradiation of visible light emitted by a 300W xenon lamp. 20 mg of the catalyst was dispersed in 100 mL of tetracycline hydrochloride solution and placed in a dark box after ultrasonic dispersion. After 30 minutes of dark reaction to reach adsorption equilibrium, the xenon lamp was turned on and 4 mL of the stock solution was taken every 15 minutes. After two centrifugations, the supernatant was placed in a cuvette and the absorbance of the liquid was tested under a UV spectrophotometer. It can be found that the degradation rate of tetracycline hydrochloride by Cu(GaCrMnFeCo)2O4 is close to 98% within 135 minutes.
[0081] Example 4
[0082] A method for preparing a Cu(AlCrMnFeCo)2O4 spinel high entropy oxide photoelectrocatalytic material, the specific steps are as follows:
[0083] (1) Accurately weigh 0.7955 g CuO, 0.2039 g Al2O3, 0.3040 g Cr2O3, 0.3477 g MnO2, 0.3194 g Fe2O3, and 0.3317 g Co2O3 metal oxide powders, transfer them to an agate mortar, add a small amount of anhydrous ethanol, and grind for 2 h to obtain powder A.
[0084] (2) Powder A is placed in a mold and pressed into a circular ceramic piece B by cold isostatic pressing.
[0085] (3) Ceramic piece B was placed in a corundum crucible and transferred to a tube furnace. The temperature was raised to 1000°C at a rate of 10°C / min in an air atmosphere and kept at that temperature for 12 h to obtain ceramic sample C.
[0086] (4) After grinding the ceramic sample C, repeat step (3) twice to obtain a high-purity spinel high-entropy oxide photoelectrocatalytic material.
[0087] Depend on Fig.18 It can be seen that under visible light irradiation, at 0V Ag / AgCl Under the voltage, the photocurrent density of Cu(AlCrMnFeCo)2O4 photoelectrode in three cycle tests was 165.5μA / cm 2 , 149.8μA / cm 2 and 146.8μA / cm 2 After three cycles of testing, the photoelectrocatalytic activity was still maintained at about 89%, and the Cu(AlCrMnFeCo)2O4 spinel high entropy oxide had good catalytic stability.
[0088] The Cu(AlCrMnFeCo)2O4 photocatalyst prepared in Example 4 exhibited excellent photocatalytic performance in decomposing water to produce hydrogen under irradiation of a 300W xenon lamp. Fig.19 It can be seen that when methanol is used as a hole sacrificial agent, 0.01 g of the photocatalyst decomposes water at a wavelength of 400 nm to produce a large amount of hydrogen, which produces a strong hydrogen signal in the gas chromatograph.
[0089] Depend on Fig. 20 It can be seen that the Cu(AlCrMnFeCo)2O4 photoelectrocatalyst prepared in this embodiment exhibits excellent photocatalytic degradation of pollutants under the irradiation of visible light emitted by a 300W xenon lamp. 20 mg of the catalyst was dispersed in 100 mL of a 10 mg / L Cr(VI) solution containing 0.2 g of diphenylcarbazide color developer powder and placed in a dark box after ultrasonic dispersion. After 15 minutes of dark reaction to reach adsorption equilibrium, the xenon lamp was turned on and 4 mL of the stock solution was taken every 5 minutes. After two centrifugations, the supernatant was placed in a cuvette and the absorbance of the liquid was tested under a UV spectrophotometer. It can be found that within 35 minutes, the Cr of Cu(AlCrMnFeCo)2O4 6+ The degradation rate can reach over 98.7%.
[0090] Example 5
[0091] A method for preparing a Cu(AlGaVCrMnFeCo)2O4 spinel high entropy oxide photoelectrocatalytic material, the specific steps are as follows:
[0092] (1) Accurately weigh 0.5569 g CuO, 0.1020 g Al2O3, 0.1874 g Ga2O3, 0.1499 g V2O3, 0.1520 g Cr2O3, 0.1739 g MnO2, 0.1597 g Fe2O3, and 0.1659 g Co2O3 metal oxide powders, transfer them to an agate mortar, add a small amount of anhydrous ethanol, and grind for 3 h to obtain powder A.
[0093] (2) Powder A is placed in a mold and pressed into a circular ceramic piece B by cold isostatic pressing.
[0094] (3) Ceramic piece B was placed in a corundum crucible and transferred to a tube furnace. The temperature was raised to 1100°C at a rate of 5°C / min in an air atmosphere and kept at this temperature for 20 h to obtain ceramic sample C.
[0095] (4) After grinding the ceramic sample C, repeat step (3) twice to obtain a high-purity spinel high-entropy oxide photoelectrocatalytic material.
[0096] Depend on Fig.21It can be seen that the Cu(AlGaVCrMnFeCo)2O4 photocatalyst exhibits excellent photocatalytic degradation of pollutants under the irradiation of visible light emitted by a 300W xenon lamp. 20mg of the catalyst was dispersed in 100mL of methyl orange solution and placed in a dark box after ultrasonic dispersion. After 20min of dark reaction to reach adsorption equilibrium, the xenon lamp was turned on and 4mL of the stock solution was taken every 10min. After two centrifugations, the supernatant was placed in a cuvette and the absorbance of the liquid was tested under a UV spectrophotometer. It can be found that the degradation rate of methyl orange by Cu(AlGaVCrMnFeCo)2O can reach more than 99% within 60min.
[0097] Depend on Fig. 22 It can be seen that when methanol is used as a hole sacrificial agent, the photocatalytic water decomposition hydrogen production rate of 0.01gCu(AlGaVCrMnFeCo)2O4 photocatalyst under visible light irradiation is about 445μmol / g / h, showing a high water decomposition hydrogen production performance, and after 3 cycles, it still maintains a water decomposition hydrogen production rate of about 441μmol / g / h, with excellent catalytic stability, and can adapt to long-term catalytic reaction tests.
[0098] Example 6
[0099] A method for preparing a Cu(AlGaCrMnFeCoNi)2O4 spinel high entropy oxide photoelectrocatalytic material, the specific steps are as follows:
[0100] (1) Accurately weigh 0.5569 g CuO, 0.1020 g Al2O3, 0.1874 g Ga2O3, 0.1520 g Cr2O3, 0.1739 g MnO2, 0.1597 g Fe2O3, 0.1659 g Co2O3, and 0.1494 g NiO metal oxide powders, transfer them to an agate mortar, add a small amount of anhydrous ethanol, and grind for 2 h to obtain powder A.
[0101] (2) Powder A is placed in a mold and pressed into a circular ceramic piece B by cold isostatic pressing.
[0102] (3) Ceramic piece B was placed in a corundum crucible and transferred to a tube furnace. The temperature was raised to 1100°C at a rate of 10°C / min in an air atmosphere and kept at that temperature for 12 h to obtain ceramic sample C.
[0103] (4) After grinding the ceramic sample C, repeat step (3) three times to obtain a high-purity spinel high-entropy oxide photoelectrocatalytic material.
[0104] The Cu(AlGaCrMnFeCoNi)2O4 photocatalyst prepared in Example 4 exhibited excellent photocatalytic performance in decomposing water to produce hydrogen under irradiation of a 300W xenon lamp. Fig.23It can be seen that when methanol is used as a hole sacrificial agent, 0.01 g of the photocatalyst decomposes water at a wavelength of 400 nm to produce a large amount of hydrogen, which produces a strong hydrogen signal in the gas chromatograph.
[0105] Depend on Fig.24 It can be seen that the Cu(AlGaCrMnFeCoNi)2O4 photoelectrocatalyst prepared in this embodiment exhibits excellent photocatalytic degradation of pollutants under the irradiation of visible light emitted by a 300W xenon lamp. 20 mg of the catalyst was dispersed in 100 mL of methylene blue solution and placed in a dark box after ultrasonic dispersion. After 20 minutes of dark reaction to reach adsorption equilibrium, the xenon lamp was turned on and 4 mL of the stock solution was taken every 10 minutes. After two centrifugations, the supernatant was placed in a cuvette and the absorbance of the liquid was tested under a UV spectrophotometer. It can be found that the degradation rate of methylene blue pollutants by Cu(AlGaCrMnFeCoNi)2O4 is close to 99% within 50 minutes.
[0106] Example 7
[0107] A method for preparing a Cu(AlGaVCrMnFeCoNi)2O4 spinel high entropy oxide photoelectrocatalytic material, the specific steps are as follows:
[0108] (1) Accurately weigh 0.5569 g CuO, 0.1020 g Al2O3, 0.1874 g Ga2O3, 0.1499 g V2O3, 0.1520 g Cr2O3, 0.1739 g MnO2, 0.1597 g Fe2O3, 0.1659 g Co2O3, and 0.1494 g NiO metal oxide powders, transfer them to an agate mortar, add a small amount of anhydrous ethanol, and grind for 0.5 h to obtain powder A.
[0109] (2) Powder A is placed in a mold and pressed into a circular ceramic piece B by cold isostatic pressing.
[0110] (3) Ceramic piece B was placed in a corundum crucible and transferred to a tube furnace. The temperature was raised to 1100°C at a rate of 5°C / min in an air atmosphere and kept at this temperature for 12 h to obtain ceramic sample C.
[0111] (4) After grinding the ceramic sample C, repeat step (3) twice to obtain a high-purity spinel high-entropy oxide photoelectrocatalytic material.
[0112] Depend on Fig.25 It can be seen that Cu(AlGaVCrMnFeCoNi)2O4 has a high photocatalytic activity for decomposing water to produce hydrogen. Under visible light irradiation, -0.4V Ag / AgCl Under the condition of2 .
[0113] Depend on Fig.26 It can be seen that under visible light irradiation, 0V Ag / AgCl Under the voltage, the photocurrent density of Cu(AlGaVCrMnFeCoNi)2O4 photoelectrode in three cycle tests was 119.1μA / cm 2 , 112.5μA / cm 2 and 102.4μA / cm 2 After three cycles of testing, the photoelectrocatalytic activity was still maintained at about 86%, indicating that the Cu(AlGaVCrMnFeCoNi)2O4 spinel high entropy oxide has good catalytic stability.
[0114] Depend on Fig. 27 It can be seen that the Cu(AlGaVCrMnFeCoNi)2O4 photocatalyst exhibits excellent photocatalytic degradation of pollutants under the irradiation of visible light emitted by a 300W xenon lamp. 20mg of the catalyst was dispersed in 100mL of tetracycline hydrochloride solution and ultrasonically dispersed and placed in a dark box. After 20min of dark reaction to reach adsorption equilibrium, the xenon lamp was turned on and 4mL of the stock solution was taken every 10min. After two centrifugations, the supernatant was placed in a cuvette and the absorbance of the liquid was tested under a UV spectrophotometer. It can be found that the degradation rate of Cu(AlGaVCrMnFeCoNi)2O4 for tetracycline hydrochloride pollutants can reach 95% within 60min, and the degradation rate of Cu(AlGaVCrMnFeCoNi)2O4 for tetracycline hydrochloride pollutants can reach 99.3% at 90min.
[0115] Comparative Example 1
[0116] A method for preparing a Cu(GaMnFe)2O4 spinel medium entropy oxide photoelectrocatalytic material, the specific steps are as follows:
[0117] (1) Accurately weigh 0.71595 g CuO, 0.5623 g Ga2O3, 0.5216 g MnO2, and 0.4791 g Fe2O3 metal oxide powders, transfer them to an agate mortar, add a small amount of anhydrous ethanol, and grind for 0.5 h to obtain powder A.
[0118] (2) Powder A is placed in a mold and pressed into a circular ceramic piece B by cold isostatic pressing.
[0119] (3) Ceramic piece B was placed in a corundum crucible and transferred to a tube furnace. The temperature was raised to 1000°C at a rate of 5°C / min in an air atmosphere and kept at this temperature for 12 h to obtain ceramic sample C.
[0120] (4) After grinding the ceramic sample C, repeat step (3) twice to obtain a high-purity spinel photoelectrocatalytic material.
[0121] Depend on Fig.28 It can be seen that under visible light irradiation, at 0V Ag / AgCl Under voltage, the photocurrent density of Cu(GaMnFe)2O4 in three cycle tests was 7μA / cm 2 , 5μA / cm 2 and 2.3μA / cm 2 The photocurrent density is much lower than that of spinel high entropy oxide photoelectrocatalytic materials. Moreover, after three cycles of testing, the photocurrent density is only 32.9% of the initial value. The catalyst undergoes obvious photodegradation, and its stability is much lower than that of spinel high entropy oxide.
[0122] Depend on Fig.29 It can be seen that the ability of Cu(GaMnFe)2O4 to degrade pollutants is much lower than that of spinel high entropy oxides. 40 mg of the catalyst was dispersed in 200 mL of tetracycline hydrochloride solution and ultrasonically dispersed and placed in a dark box. After 30 minutes of dark reaction to reach adsorption equilibrium, the xenon lamp was turned on and 4 mL of the stock solution was taken every 10 minutes. After two centrifugations, the supernatant was placed in a cuvette and the absorbance of the liquid was tested under a UV spectrophotometer. Within 3 hours, the degradation rate of tetracycline hydrochloride pollutants by Cu(GaMnFe)2O4 was 96.5%, and the degradation rate was much lower than that of high entropy oxides.
[0123] Depend on Fig.30 It can be seen that the photocatalytic decomposition of water and hydrogen production rate of Cu(GaMnFe)2O4 photocatalyst is much lower than that of spinel high entropy oxides. When methanol is used as a hole sacrificial agent, the decomposition of water and hydrogen production rate of 0.01gCu(GaMnFe)2O4 under visible light irradiation is only 3.72μmol / g / h.
[0124] Comparative Example 2
[0125] A method for preparing a CuFe2O4 spinel photoelectrocatalytic material, the specific steps are as follows:
[0126] (1) Accurately weigh 0.79545 g CuO and 1.5969 g Fe2O3 metal oxide powders, transfer them to an agate mortar, add a small amount of anhydrous ethanol and continue grinding for 0.5 h to obtain powder A.
[0127] (2) Powder A is placed in a mold and pressed into a circular ceramic piece B by cold isostatic pressing.
[0128] (3) Ceramic piece B was placed in a corundum crucible and transferred to a tube furnace. The temperature was raised to 1000°C at a rate of 5°C / min in an air atmosphere and kept at this temperature for 12 h to obtain ceramic sample C.
[0129] (4) After grinding the ceramic sample C, repeat step (3) twice to obtain a high-purity spinel high-entropy oxide photoelectrocatalytic material.
[0130] like Fig.31 As shown in Figure 2, the photoelectrocatalytic performance of CuFe2O4 spinel low entropy oxide is much lower than that of high entropy oxide. Under the irradiation of a 300W xenon lamp, the photocurrent density of CuFe2O4 is only 0.36μA / cm 2 , much lower than high entropy oxides.
[0131] like Fig.32 As shown in the figure, under visible light irradiation, after 300 minutes of reaction, the degradation rate of tetracycline hydrochloride by CuFe2O4 is 96%. The ability of CuFe2O4 spinel low entropy oxide to degrade pollutants is much lower than that of high entropy oxide, and the stability of CuFe2O4 spinel low entropy oxide is poor, and Fe is easily leached.
[0132] like Fig.33 As shown in the figure, when methanol is used as a hole sacrificial agent, the hydrogen production rate of 0.01g CuFe2O4 photocatalytic water decomposition under visible light irradiation is only 1.65μmol / g / h, which is much lower than that of spinel high entropy oxide. In addition, due to the low hydrogen production performance, the hydrogen production in the first two hours is lower than the detection limit of gas chromatography, and no characteristic peak of H2 is detected.
[0133] Low entropy oxides contain only two metal ions, Cu and Fe, and have poor charge transfer capabilities, which makes their carrier separation efficiency and transfer rate lower than those of high entropy oxides. In addition, there are fewer active sites in CuFe2O4, and the reactants cannot be adsorbed on the catalyst, so that many photogenerated carriers cannot participate in the reaction and recombine in the bulk phase, reducing the catalytic reaction activity. In addition, the inappropriate energy band structure of CuFe2O4 is also the reason why its performance is far lower than that of high entropy oxides.
[0134] Comparative Example 3
[0135] A method for preparing a Cu(GaCrMnFeCoNi)2O4 spinel high entropy oxide photoelectrocatalytic material, the specific steps are as follows:
[0136] (1) Accurately weigh 0.7955 g CuO, 0.313 g Ga2O3, 0.2538 g Cr2O3, 0.2904 g MnO2, 0.2667 g Fe2O3, 0.277 g Co2O3, and 0.2495 g NiO metal oxide powders, transfer them to an agate mortar, add a small amount of anhydrous ethanol, and grind for 2 h to obtain powder A.
[0137] (2) Powder A is placed in a mold and pressed into a circular ceramic piece B by cold isostatic pressing.
[0138] (3) The ceramic sheet B was placed in a corundum crucible and transferred to a tubular furnace. The temperature was raised to 1000°C at a rate of 5°C / min in an air atmosphere and kept at this temperature for 30 h to obtain a high-purity spinel high-entropy oxide photoelectrocatalytic material.
[0139] like Fig.34 As shown, the Cu(GaCrMnFeCoNi)2O4 prepared by one-step sintering contains a large amount of CuO impurities in addition to spinel oxide, and XRD shows that CuO accounts for about 59.28wt%. In the case of only one sintering, a mixture of high entropy oxide (CuGaCrMnFeCoNi)3O4 and CuO with a spinel phase is formed instead of a single spinel high entropy oxide with a space group of I41 / amd. Multi-step sintering is required to make the raw material undergo a phase change to form a Cu(GaCrMnFeCoNi)2O4 spinel high entropy oxide with a space group of I41 / amd.
[0140] Comparative Example 4
[0141] A method for preparing a Cu(VCrMnFeCo)2O4 spinel high entropy oxide photoelectrocatalytic material, the specific steps are as follows:
[0142] (1) Accurately weigh 0.3977 g CuO, 0.1499 g V2O3, 0.1520 g Cr2O3, 0.1739 g MnO2, 0.1597 g Fe2O3, and 0.1659 g Co2O3 metal oxide powders, transfer them to an agate mortar, add a small amount of anhydrous ethanol, and grind for 1.5 h to obtain powder A.
[0143] (2) Powder A is placed in a mold and pressed into a circular ceramic piece B by cold isostatic pressing.
[0144] (3) Ceramic piece B was placed in a corundum crucible and transferred to a tube furnace. The temperature was raised to 1100°C at a rate of 10°C / min in an air atmosphere and kept at that temperature for 12 h to obtain ceramic sample C.
[0145] (4) After grinding the ceramic sample C, repeat step (3) three times to obtain a high-purity spinel high-entropy oxide photoelectrocatalytic material.
[0146] like Fig.35 As shown, the samples prepared without adding Al or Ga elements contain not only spinel oxides belonging to the Fd-3m space group, but also impurities belonging to delafossite-type oxides and Cu oxides, and pure spinel high-entropy oxides cannot be prepared.
[0147] Comparative Example 5
[0148] A method for preparing a Cu(GaCrMnFeCoBi)2O4 spinel high entropy oxide photoelectrocatalytic material, the specific steps are as follows:
[0149] (1) Accurately weigh 0.4773 g CuO, 0.1875 g Ga2O3, 0.1520 g Cr2O3, 0.1739 g MnO2, 0.1597 g Fe2O3, 0.1659 g Co2O3, and 0.4660 g Bi2O3 metal oxide powders, transfer them to an agate mortar, add a small amount of anhydrous ethanol, and grind for 3 h to obtain powder A.
[0150] (2) Powder A is placed in a mold and pressed into a circular ceramic piece B by cold isostatic pressing.
[0151] (3) Ceramic piece B was placed in a corundum crucible and transferred to a tube furnace. The temperature was raised to 1150°C at a rate of 5°C / min in an air atmosphere and kept at this temperature for 12 h to obtain ceramic sample C.
[0152] (4) After grinding the ceramic sample C, repeat step (3) three times to obtain a high-purity spinel high-entropy oxide photoelectrocatalytic material.
[0153] like Fig.36 As shown, in the presence of other elements, such as metal elements other than the fourth period elements (such as Bi), the prepared high entropy oxide contains, in addition to the spinel oxide belonging to the Fd-3m space group, also numerous impurity compounds such as ferroxite oxide and Bi2O3, and pure spinel high entropy oxide cannot be obtained.
[0154] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A spinel high entropy oxide photoelectrocatalytic material, characterized in that: The chemical formula is CuM2O4, the crystal structure is spinel structure, tetragonal body-centered unit cell, belongs to tetragonal crystal system, and the space group is I41 / amd; M is 5-8 of Al, Ga, V, Cr, Mn, Fe, Co, Ni elements, and the molar percentage of each M element is 10-20%; Wherein M contains at least one of Al and Ga; The method for preparing the spinel-type high entropy oxide photoelectrocatalytic material comprises: mixing copper oxide and an oxide of metal M and sintering the mixture to obtain the spinel-type high entropy oxide photoelectrocatalytic material.
2. The spinel high entropy oxide photoelectrocatalytic material according to claim 1, characterized in that: The spinel-type high entropy oxide photoelectrocatalytic material is a single spinel structure.
3. The spinel high entropy oxide photoelectrocatalytic material according to claim 1, characterized in that: The heating method used for sintering is radiation heating.
4. The spinel high entropy oxide photoelectrocatalytic material according to claim 1, characterized in that: The sintering temperature is 900-1200° C., the sintering time is 4-30 hours, and the atmosphere is oxygen or air.
5. The spinel high entropy oxide photoelectrocatalytic material according to claim 1, characterized in that: The sintering times are more than 3 times.
6. Use of the spinel high entropy oxide photoelectrocatalytic material according to any one of claims 1 to 5 in photocatalytic hydrolysis to produce hydrogen.
7. Use of the spinel high entropy oxide photoelectrocatalytic material according to any one of claims 1 to 5 in the removal of organic pollutants or heavy metals.
Citation Information
Cited By
Preparation method and application of BiVO4 / CuFe2O4 composite photo-anode
CN119913559A