Non-noble metal phosphide catalyst as well as preparation method and application thereof
By preparing the non-precious metal phosphide catalyst Ni-FeCoP in electrolytic water, the problem of insufficient electrochemical performance and stability of non-precious metal phosphide materials in the prior art is solved, and the effect of efficient catalyzing of oxygen production reaction in electrolytic water is achieved.
Patent Information
- Application Number
- CN202411028197.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art has not yet effectively improved the electrochemical performance and stability of non-precious metal phosphide materials, especially in the oxygen production reaction in electrolytic water.
By adding urea and ammonium fluoride to the mixed aqueous solution of cobalt nitrate and ferric nitrate, iron-cobalt dihydroxide compound is formed, and ion exchange is performed and calcined with sodium hypophosphite is performed to prepare the non-precious metal phosphide catalyst Ni-FeCoP, and the Large surface roughness and form heterojunctions to improve electrochemical properties.
It significantly improves the electrochemical performance of the catalyst, including lower overpotential and higher stability. Ni-FeCoP catalyst can effectively catalyze oxygen production reactions in electrolyzed water, with better performance than previous catalysts and good theoretical research. Value and application prospects.
Smart Images

Figure CN118932378A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of electrocatalysis technology, and in particular to a non-noble metal phosphide catalyst and a preparation method and application thereof. Background Art
[0002] In the field of water electrolysis, hydrogen production by water electrolysis (HER) has a smaller energy requirement than oxygen production by water electrolysis (OER), so OER is the main obstacle to the entire water electrolysis. Although researchers have developed ruthenium oxide and iridium oxide as catalysts for efficient OER, the high cost and scarcity of precious metals have led to their narrow application. Therefore, it is necessary to design low-cost, highly stable and highly active catalysts.
[0003] At present, researchers have devoted a lot of energy to non-precious metal catalysts, such as metal oxides, transition metal sulfides, transition metal hydroxides, etc. Among them, transition metal phosphides (TMPs) have attracted much attention because of their unique hydrogenase-like catalytic mechanism, which produces high water decomposition catalytic activity. The role of P in TMPs is also reflected in the embedded transition metal lattice increasing the atomic distance, thereby weakening the interaction between metals, changing the d-band center, and affecting the adsorption of intermediates. Secondly, metal phosphides can inhibit metal dissolution from a thermodynamic point of view, thereby improving the corrosion resistance and stability of the catalyst.
[0004] However, the current technology for modifying phosphide metal catalysts to improve performance and stability still has certain difficulties. The technology for modifying non-precious metal phosphides is an important processing method. According to different modification methods, different effects (HER, OER) can be provided in the field of water electrolysis. For example, the existing patent CN117822031A discloses a phosphide hydrogen evolution catalyst with a built-in electric field and its preparation method and application. The patent grows nickel-cobalt precursor nanowires in situ on a nickel foam substrate, and then transforms them into nickel phosphide / cobalt phosphide nanowires with a built-in electric field through simple low-temperature phosphating, which are efficiently used for hydrogen evolution reactions. Another example is the existing patent CN116837406A discloses a nickel phosphide substrate-loaded iron-cobalt oxide electrolysis seawater oxygen evolution catalyst and its preparation and application. The patent exhibits ultra-long-term stability in seawater electrolysis, and has the advantages of mild preparation conditions, simple process flow, low energy consumption, batch-to-batch repeatability and reduced reaction overpotential. Its performance is 100mA / cm -2 The overpotential reached 246 mV, which is still insufficient, but its excellent stability shows that metal phosphides are expected to be widely used in the field of electrocatalytic decomposition of seawater to produce hydrogen. Summary of the invention
[0005] The purpose of the present invention is to provide a non-precious metal phosphide catalyst and its preparation method and application in order to overcome the problem that the prior art is not yet compatible with improving the electrochemical performance and stability of non-precious metal phosphide materials.
[0006] The purpose of the present invention can be achieved by the following technical solutions:
[0007] One of the technical solutions of the present invention is to provide a method for preparing a non-precious metal phosphide catalyst, comprising the following steps:
[0008] S1. Add urea and ammonium fluoride to a mixed aqueous solution of cobalt nitrate and ferric nitrate, and heat the mixture in stages to react to obtain iron-cobalt double hydroxide FeCo-LDH;
[0009] S2, immersing the iron-cobalt double hydroxide FeCo-LDH obtained in step S1 in a nickel nitrate aqueous solution for ion exchange to obtain Ni-FeCo-LDH;
[0010] S3. Under an inert atmosphere, the Ni-FeCo-LDH obtained in step S2 is calcined with sodium hypophosphite to carry out a phosphating reaction to obtain a non-precious metal phosphide catalyst Ni-FeCoP.
[0011] In some specific embodiments, in step S1, the concentration of cobalt nitrate in the mixed aqueous solution of cobalt nitrate and ferric nitrate is (0.016-0.017)M, and the concentration of ferric nitrate is (0.03-0.04)M.
[0012] In some specific embodiments, in step S1, the molar ratio of urea, sodium fluoride, ferric nitrate and cobalt nitrate is 30:15:2:1.
[0013] In some specific embodiments, in step S1, the staged heating steps are: first heating to 110-120° C. and keeping warm for 3 hours; then heating to 150-160° C. and keeping warm for 3 hours.
[0014] In some specific embodiments, in step S2, the concentration of nickel nitrate in the nickel nitrate aqueous solution is (0.4-0.6) M, and the molar ratio of nickel nitrate to iron nitrate in the nickel nitrate aqueous solution is (400-600):1.
[0015] In some specific embodiments, in step S2, the reaction temperature of ion exchange is 18-30° C., and the reaction time is 40 min.
[0016] In some specific embodiments, in step S3, the molar ratio of sodium hypophosphite to ferric nitrate is (18-19):1.
[0017] In some specific embodiments, in step S3, the inert atmosphere is nitrogen, and the phosphating reaction conditions are heating to 300° C. at a heating rate of 5° C. / min and keeping the temperature for 2 h.
[0018] A second technical solution of the present invention is to provide a non-precious metal phosphide catalyst, based on the preparation method described in one of the above technical solutions.
[0019] A third technical solution of the present invention is to provide an application of the non-precious metal phosphide catalyst as described in the second technical solution above, wherein the non-precious metal phosphide catalyst is applied to electrocatalytic oxygen production.
[0020] In some specific embodiments, the non-precious metal phosphide catalyst is used for electrocatalytic oxygen production in an alkaline electrolyte.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] (1) The present invention creatively exchanges Ni ions with iron-cobalt double hydroxide FeCo-LDH, thereby increasing the surface roughness and exposing more active sites. Then, in the phosphating reaction, PH3 produced by sodium hypophosphite is used to phosphide metal iron, cobalt and nickel to form a heterojunction, thereby effectively improving the electrochemical performance of the prepared non-precious metal phosphide catalyst Ni-FeCoP.
[0023] (2) The non-precious metal phosphide catalyst Ni-FeCoP prepared by the present invention can be effectively used as a catalyst for the oxygen evolution reaction at the anode of water electrolysis.
[0024] (3) The non-precious metal phosphide prepared by ion exchange provided by the present invention has good theoretical research value and provides a new idea for effectively improving the electrochemical performance of phosphide electrocatalytic oxygen production, thereby further broadening the application prospects of this method in the field of electrochemical oxygen (hydrogen) production. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 These are the XRD patterns of FeCo-LDH-1 and FeCo-LDH-2.
[0026] Figure 2 This is the XRD pattern of Ni-FeCoP-2.
[0027] Figure 3 LSV (after IR85% compensation) of Ni-FeCoP-2, Ni-FeCoP-1, FeCo-LDH-1, and FeCo-LDH-2.
[0028] Figure 4Tafel diagrams of Ni-FeCoP-2, Ni-FeCoP-1, FeCo-LDH-1, and FeCo-LDH-2.
[0029] Figure 5 Cdl diagram of Ni-FeCoP-2, Ni-FeCoP-1, FeCo-LDH-1, and FeCo-LDH-2.
[0030] Figure 6 These are the EIS diagrams of Ni-FeCoP-2, Ni-FeCoP-1, FeCo-LDH-1, and FeCo-LDH-2.
[0031] Figure 7 This is the chronoamperometry diagram of Ni-FeCoP-2.
[0032] Figure 8 This is the SEM image of FeCo-LDH-1.
[0033] Fig. 9 This is the SEM image of FeCo-LDH-2.
[0034] Fig.10 This is the SEM image of Ni-FeCoP-1.
[0035] Fig.11 This is the SEM image of Ni-FeCoP-2. DETAILED DESCRIPTION
[0036] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.
[0037] In the following examples and comparative examples, unless otherwise specified, raw materials or processing techniques are conventional commercially available raw materials or conventional processing techniques in the art.
[0038] Embodiment 1:
[0039] This embodiment provides a non-precious metal phosphide catalyst Ni-FeCoP-2 grown in situ on nickel foam, and the preparation method comprises the following steps:
[0040] (1) First, 30% hydrochloric acid solution and acetone are used to clean the NF (nickel foam) to remove oxides and oils.
[0041] (2) Then, the nickel foam was immersed in a 30 mL aqueous solution of 0.404 g Fe(NO3)3·9H2O and 0.145 g Co(NO3)2·6H2O, and 0.9009 g urea and 0.2777 g ammonium fluoride were added in sequence. The mixture was placed in a 100 mL hydrothermal kettle and heated to 120°C for 3 hours, and then heated to 160°C for 3 hours. After the reaction, it was naturally cooled and washed alternately with ethanol and deionized water, and vacuum dried at 60°C to obtain iron-cobalt double hydroxide FeCo-LDH, named FeCo-LDH-2.
[0042] (3) 1.454 g Ni(NO3)2·6H2O was dissolved in 10 mL water by ultrasonication, and FeCo-LDH-2 was immersed in the solution and kept at room temperature for 40 min. After being taken out, it was vacuum-dried at 60 °C to obtain Ni-FeCo-LDH-2.
[0043] (4) The dried Ni-FeCo-LDH-2 was placed in the middle of a tubular furnace filled with nitrogen, and 2 g of sodium hypophosphite monohydrate was placed upstream of the tubular furnace. Both were loaded in a porcelain boat, and the temperature was raised to 300 °C at a rate of 5 °C / min and kept at this temperature for 2 hours to obtain a non-precious metal phosphide catalyst Ni-FeCoP-2.
[0044] Comparative Example 1:
[0045] Compared with Example 1, most of the steps are the same, except that the step of heating to 160° C. for 3 hours is omitted. The specific steps are as follows:
[0046] (1) First, 30% hydrochloric acid solution and acetone are used to clean the NF (nickel foam) to remove oxides and oils.
[0047] (2) Then, the nickel foam was immersed in 0.404g Fe(NO3)3·9H2O and 0.145g Co(NO3)2·6H2O in a 30ml aqueous solution, and 0.9009g urea and 0.2777g ammonium fluoride were added in sequence. The mixture was placed in a 100mL hydrothermal autoclave and heated to 120°C for 3 hours. After the reaction, it was cooled naturally and washed alternately with ethanol and deionized water, and dried in a vacuum oven at 60°C to obtain an iron-cobalt double hydroxide FeCo-LDH, which was named FeCo-LDH-1.
[0048] (3) 1.454 g Ni(NO3)2·6H2O was dissolved in 10 mL water by ultrasonication, and FeCo-LDH-1 was immersed in the solution and kept at room temperature for 40 min. After being taken out, it was vacuum-dried at 60 °C to obtain Ni-FeCo-LDH-1.
[0049] (4) The dried Ni-FeCo-LDH-1 was placed in the middle of a tubular furnace filled with nitrogen, and 2 g of sodium hypophosphite monohydrate was placed upstream of the tubular furnace. Both were loaded in a porcelain boat, and the temperature was raised to 300 °C at a rate of 5 °C / min and kept at this temperature for 2 hours to obtain a non-precious metal phosphide catalyst Ni-FeCoP-1.
[0050] like Figure 1 , are the XRD patterns of FeCo-LDH-1 and FeCo-LDH-2. Figure 1 It can be clearly seen that the FeCo-LDH-2 obtained by stage heating has the same XRD peak value as the FeCo-LDH-1 prepared by the conventional scheme of Comparative Example 1, indicating that no new phase is generated in the material during the stage heating process.
[0051] like Figure 2 , is the XRD pattern of Ni-FeCoP-2, from Figure 2 It can be seen that the XRD peaks of Ni-FeCoP-2, the product obtained by low-temperature phosphating of FeCo-LDH-2, correspond to Ni2P, Fe2P, and Co2P, and transition metal phosphides are successfully formed on the surface.
[0052] like Figure 8-11 As shown, the SEM images of FeCo-LDH-1, FeCo-LDH-2, Ni-FeCoP-1, and Ni-FeCoP-2 are shown. Figure 8 and Fig. 9 From the SEM images of FeCo-LDH-1 and FeCo-LDH-2, it can be clearly seen that a hierarchical spatial structure is generated by the staged heating, which is formed by the accumulation of layers of FeCo-LDH on the FeCo-LDH-1 sheet, thereby generating more active sites. In contrast, it can be clearly seen that FeCo-LDH-1 has significantly fewer exposed active sites. Fig.10 and Fig.11 The SEM images of Ni-FeCoP-1 and Ni-FeCoP-2 show that Ni-FeCoP-2 retains the original hierarchical spatial structure, indicating that the phosphating calcination process will not cause the hierarchical spatial structure to aggregate and collapse. At the same time, based on this structure, Ni-FeCoP-2 has a better electrochemical active surface area than Ni-FeCoP-1 ( Figure 5 ),performance( Figure 3 ), since FeCo-LDH-2 was successfully doped with nickel, a large number of particles were formed on the surface of the material.
[0053] The Ni-FeCoP-1 and Ni-FeCoP-2 prepared above were subjected to the following performance tests:
[0054] Using graphite as the counter electrode, mercury / mercury oxide as the reference electrode, and platinum electrode as the working electrode, the nickel foam on which the catalyst was grown was sandwiched between the platinum electrode to ensure that the platinum was in close contact with the nickel foam. The catalyst was then activated by cyclic voltammetry using Shanghai Chenhua electrochemical workstation 760E in an H-type electrolytic cell filled with 1M KOH electrolyte.
[0055] Cyclic voltammetry was performed at 0-0.7V, with a scan rate of 100mV / s for 40 cycles, and then linear sweep voltammetry was tested at a rate of 5mV / s in the same potential range. Finally, the open circuit voltage was used to automatically perform IR compensation to obtain a performance graph to eliminate the influence of solution resistance and instrument resistance.
[0056] The stability test is carried out using a chronoamperometric test at 100 mA / cm -2 The potential change under Figure 7 Chronoamperometry diagram of Ni-FeCoP-2.
[0057] like Figure 3 , is the LSV diagram of the polarization curves of Ni-FeCoP-2, Ni-FeCoP-1, FeCo-LDH-1, and FeCo-LDH-2 (after IR85% compensation), from Figure 3 It can be seen that the OER performance of Ni-FeCoP-2 is 100 mA cm -2 The overpotential reached 175 mV at 1 A cm -2 The catalyst achieves 285 mV at a high current density, which is significantly better than other catalysts studied in the experiment.
[0058] like Figure 4 , are the Tafel plots of Ni-FeCoP-2, Ni-FeCoP-1, FeCo-LDH-1, and FeCo-LDH-2. Ni-FeCoP-2 shows a lower Tafel slope, indicating that the reaction kinetics of the Ni-FeCoP-2 catalyst is faster and the catalytic activity is better.
[0059] like Figure 5 , is the double layer capacitance Cdl diagram of Ni-FeCoP-2, Ni-FeCoP-1, FeCo-LDH-1, and FeCo-LDH-2. The larger slope of Ni-FeCoP-2 indicates that it has a larger capacitance, so Ni-FeCoP-2 has more active surface area, which proves the reason why Ni-FeCoP-2 catalyst has excellent performance.
[0060] like Figure 6, are the electrochemical impedance spectroscopy (EIS) graphs of Ni-FeCoP-2, Ni-FeCoP-1, FeCo-LDH-1, and FeCo-LDH-2. The smaller impedance semicircle indicates that Ni-FeCoP-2 has smaller resistance and greater ion transport, which once again proves the reason for the excellent performance of Ni-FeCoP-2 catalyst.
[0061] like Figure 7 , is the current diagram of Ni-FeCoP-2, from Figure 7 It can be seen that Ni-FeCoP-2 has a -2 It can be stable for 2000h.
[0062] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A method for preparing a non-precious metal phosphide catalyst, characterized in that: The steps include: S1. Add urea and ammonium fluoride to a mixed aqueous solution of cobalt nitrate and ferric nitrate, and heat the mixture in stages to react to obtain iron-cobalt double hydroxide FeCo-LDH; S2, immersing the iron-cobalt double hydroxide FeCo-LDH obtained in step S1 in a nickel nitrate aqueous solution for ion exchange to obtain Ni-FeCo-LDH; S3. Under an inert atmosphere, the Ni-FeCo-LDH obtained in step S2 is calcined with sodium hypophosphite to carry out a phosphating reaction to obtain a non-precious metal phosphide catalyst Ni-FeCoP.
2. The method for preparing a non-precious metal phosphide catalyst according to claim 1, characterized in that: In step S1, the concentration of cobalt nitrate in the mixed aqueous solution of cobalt nitrate and ferric nitrate is (0.016-0.017) mM, and the concentration of ferric nitrate is (0.03-0.04) mM.
3. The method for preparing a non-precious metal phosphide catalyst according to claim 1, characterized in that: In step S1, the molar ratio of urea, sodium fluoride, ferric nitrate and cobalt nitrate is 30:15:2:
1.
4. The method for preparing a non-precious metal phosphide catalyst according to claim 1, characterized in that: In step S1, the step of stage heating is: first heating to 110-120°C and keeping warm for 3 hours; then heating to 150-160°C and keeping warm for 3 hours.
5. The method for preparing a non-precious metal phosphide catalyst according to claim 1, characterized in that: In step S2, the concentration of nickel nitrate in the nickel nitrate aqueous solution is (0.4-0.6) M, and the molar ratio of nickel nitrate to iron nitrate in the nickel nitrate aqueous solution is (400-600):
1.
6. The method for preparing a non-precious metal phosphide catalyst according to claim 1, characterized in that: In step S2, the reaction temperature of the ion exchange is 18-30° C., and the reaction time is 40 min.
7. The method for preparing a non-precious metal phosphide catalyst according to claim 1, characterized in that: In step S3, the molar ratio of sodium hypophosphite to ferric nitrate is (18-19):
1.
8. The method for preparing a non-precious metal phosphide catalyst according to claim 1, characterized in that: In step S3, the inert atmosphere is nitrogen, and the phosphating reaction conditions are heating to 300° C. at a heating rate of 5° C. / min and keeping the temperature for 2 h.
9. A non-precious metal phosphide catalyst, characterized in that: Obtained based on the preparation method described in any one of claims 1-8.
10. Use of the non-precious metal phosphide catalyst as claimed in claim 9, characterized in that: The non-noble metal phosphide catalyst is used for electrocatalytic oxygen production.
Citation Information
Cited By
Sulfur-resistant methane dry reforming catalyst as well as preparation method and application thereof
CN119657148A