Cyclic utilization method of alkaline ore pulp electrolyte

By adjusting the electrolyte parameters in the alkaline slurry electrolytic method, the recycling of electrolyte is realized, the difficulty of recycling of alkaline slurry electrolyte is solved, the recycling of high-purity copper and high current efficiency is achieved, and chemical reagents and solids are reduced. The use of waste has promoted the high-value resource recycling of used mobile phone circuit boards.

CN118932425APending Publication Date: 2024-11-12SOUTHWEAT UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310516109.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing technology is difficult to realize the recycling of alkaline slurry electrolyte, which hinders the industrialization of metal recycling in waste mobile phone circuit boards.

Method used

The ammonia-ammonium chloride alkaline slurry electrolysis method is used to adjust the pH value and ion concentration of the electrolyte after the first electrolysis, and the recycling of the electrolyte is achieved, selective deposition and recovery of high-purity copper, reducing the use of chemical reagents and the generation of solid waste.

Benefits of technology

Realizes high purity recycling of copper in waste mobile phone circuit boards (more than 99.9%) and high current efficiency (more than 90%), reduces the use of chemical reagents and solid waste generation, saves costs, protects the environment, and is the industrialization of alkaline slurry electrolysis. Recycling reference is provided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932425A_ABST
    Figure CN118932425A_ABST
Patent Text Reader

Abstract

The invention discloses a cyclic utilization method of an alkaline ore pulp electrolyte. According to the method, copper can be selectively extracted from an ammonia solution, and under the condition that a copper (II) ammine complex can react with metal copper in principle to generate a copper (I) ammine complex, high-purity copper is recycled from WPCB-MPs through electrolyte circulation. According to the method, deposition and recovery of copper are selectively achieved, generation of solid waste is reduced, and in the recovery process, use of chemical reagents is reduced, so that cost is saved, the environment is protected, and reference is provided for high-value resource recycling of waste circuit boards through electrolysis of alkaline ore pulp.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a slurry electrolytic copper smelting technology, and in particular to a recycling method for alkaline slurry electrolyte. Background Art

[0002] Circuit board is one of the core components in mobile phones. The generation of used mobile phones is accompanied by a large number of waste printed circuit boards of mobile phones (WPCB-MPs). WPCB-MPs contain a large amount of non-ferrous metals such as copper, tin, lead, and nickel, and are the most valuable secondary resources in mobile phone components. Therefore, the recovery of metals in WPCB-MPs has always been a hot topic of research. At present, the metal recovery methods of WPCB-MPs mainly include mechanical and physical methods, pyrometallurgy, hydrometallurgy and biometallurgy. Traditional hydrometallurgy mainly uses strong acid or strong alkali to leach metals from waste circuit boards, then separates the leachate to remove impurities, and finally obtains the target metal through purification, precipitation, filtration, extraction, ion exchange and other methods. Slurry electrolysis is a special hydrometallurgical technology that combines metal leaching, partial solution purification and electrodeposition in one device, so it has significant advantages such as short process, low energy consumption, good metal separation effect and environmental protection. Studies have shown that in an ammonia-ammonium chloride alkaline slurry electrolysis system, Cu can form a low-valent [Cu(NH3)2] + Copper-ammonia complexes are thus deposited at the cathode, while metals such as iron and manganese can hardly form such complexes, which helps to improve current efficiency and copper purity. After long-term research by the research team, it has been confirmed that ammonia-ammonium chloride alkaline slurry electrolysis is an effective method for recovering metals from waste mobile phone circuit boards. Electrolyte circulation can reduce the use of chemical reagents and the generation of waste liquid, save costs, protect the environment, and plays an important role in industrial production. However, how to achieve electrolyte circulation during the electrolysis process has become a key factor hindering the industrial development of alkaline slurry electrolysis. In response to the above-mentioned new WPCB-MPs resource technology, finding a method suitable for the circulation of ammonia-ammonium chloride alkaline slurry electrolyte is a technical problem that needs to be solved urgently to achieve the industrialization of alkaline slurry electrolysis. Summary of the invention

[0003] The object of the present invention is to provide a method for recycling alkaline slurry electrolyte.

[0004] In order to achieve the above object, the technical solution adopted by the present invention is as follows: a method for recycling alkaline slurry electrolyte, comprising at least the following steps:

[0005] S1. Prepare an alkaline slurry electrolyte containing a certain concentration, add WPCB-MPs powder, and perform the first electrolysis at a certain current density;

[0006] S2. After the first electrolysis is completed, the electrolyte is filtered and the separated electrolyte is adjusted to the following parameters before continuing the cyclic electrolysis. The parameters are: adjusting the pH of the electrolyte to 9.80-10.0 with ammonia water, adjusting the NH4 in the electrolyte with NH4Cl + The molar concentration of the substance is 40-42g / L, and CuSO4·H2O is used to adjust the Cu in the electrolyte. 2+ The concentration is 20g / L.

[0007] Preferably, the alkaline slurry electrolyte includes 0.5 mol / L NaCl, 0.5 mol / L NH4Cl, 4 mol / L NH3·H2O, 20 g / L Cu 2+ .

[0008] Preferably, the WPCB-MPs powder is obtained by manually disassembling the waste mobile phone circuit boards to remove components, then crushing them with a cutting crusher, and passing through a 40-mesh sieve.

[0009] Preferably, the current density is 15-20 mA / cm 2 , preferably 20mA / cm 2 ; The electrolysis time is 4-6h, preferably 4h.

[0010] Preferably, the solid-liquid ratio during electrolysis (i.e., the ratio of WPCB-MPs powder to electrolyte) is 30 g / L. Compared with the prior art, the present invention has the following advantages:

[0011] (1) In an ammonia solution, copper can be selectively extracted, and copper (II) ammine complexes can in principle react with metallic copper to form copper (I) ammine complexes, thereby promoting current efficiency and purity. Therefore, ammonia-ammonium chloride alkaline slurry electrolysis has been proven to be an effective method for recovering metals from waste printed circuit boards (WPCBs). On this basis, the use of electrolyte reuse to recover high-purity copper from waste mobile phone printed circuit boards (WPCB-MPs) not only selectively achieves copper deposition recovery and reduces the generation of solid waste; but also reduces the use of chemical reagents during the recovery process, thereby saving costs and protecting the environment, providing a reference for the high-value resource recycling of waste circuit boards using alkaline slurry electrolysis.

[0012] (2) The present invention proves that ammonia-ammonium chloride alkaline slurry electrolysis can realize electrolyte circulation. In each electrolysis, the purity of the recovered cathode copper foil is higher than 99.9%, the copper recovery rate in the waste mobile phone circuit board is higher than 90%, and the current efficiency is basically higher than 90%. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 The present invention is a process flow chart of a method for recycling metallic copper from waste mobile phone circuit boards by reusing alkaline slurry electrolyte.

[0014] Figure 2 The results are the recovery rate, cathode product copper purity (a) and current efficiency (b) of Example 2 of the present invention.

[0015] Figure 3 This is a comparison chart of the recovery rate, cathode product copper purity, and current efficiency of Comparative Example 1. DETAILED DESCRIPTION

[0016] The present invention is further described below in conjunction with the accompanying drawings and embodiments.

[0017] The present invention adopts ammonia-ammonium chloride alkaline slurry electrolysis method to directly recover metallic copper from waste mobile phone circuit boards, and Cu can form low-valent [Cu(NH3)2] + The copper ammonia complex is thus deposited at the cathode, while metals such as iron and manganese can hardly form such complexes, which helps to improve the current efficiency and copper purity, and its purity reaches 99.99%. After the first electrolysis, the copper concentration in the electrolyte is 20.51g / L (equivalent to the initial copper concentration), indicating that the electrolyte can continue to be recycled after proper optimization. The present invention finds a suitable electrolyte optimization method, and multiple uses not only selectively realize copper deposition recovery and reduce the generation of solid waste, but also reduce the use of chemical reagents in the recycling process, thereby saving costs and protecting the environment, providing a reference for the high-value resource recycling of waste circuit boards in alkaline slurry electrolysis.

[0018] Waste mobile phone circuit boards were purchased from a waste home appliance recycling station. In addition to the substrate, the circuit boards also include pads, vias, mounting holes, wires, components, etc. Dismantling them is not only conducive to crushing, but also conducive to classified resource recovery. The main purpose of the present invention is to recover copper in WPCB-MPs. Therefore, it is necessary to remove the components in the waste mobile phone circuit boards to reduce the content of other metals in the original sample, thereby avoiding interference with Cu during the recycling process. After manual physical disassembly of WPCB-MPs, there are no electronic components. First, they are cut into blocks with scissors, and then crushed by a cutting crusher. After multiple crushing and screening (40 mesh), waste mobile phone board powder with a particle size of <0.45mm is obtained. The crushed samples are dried at 60°C for 24 hours and stored for standby. The main component of the waste mobile phone board powder is copper. Combined with ICP-OES and XRF determination, the copper content is 34.38%.

[0019] Example 1

[0020] In this embodiment, the metal copper in the waste mobile phone circuit board is recycled by alkaline slurry electrolyte. The process is as follows: Figure 1 shown.

[0021] (1) The first electrolysis electrolyte was 200 mL, 0.5 mol / L NaCl, 0.5 mol / L NH4Cl, 4 mol / L NH3·H2O, 20 g / L Cu 2+ (CuSO4·5H2O). Add 6g WPCB-MPs powder into the anode chamber, stir, 20mA / cm 2 Electrolysis was performed for 3 hours. After the electrolysis was completed, the copper foil in the cathode area was collected and repeatedly rinsed with a 1:2 ammonia water mixture to wash away the copper-ammine complex on the surface of the copper foil. After washing, it was dried at 60°C to constant weight. The slurry was filtered through a 0.45μm porous filter membrane, and the anode slag was dried at 60°C to constant weight. The separated electrolyte was used for the second cycle. For the second electrolysis, the remaining electrolyte after the first electrolysis was used, and the pH of the electrolyte was adjusted to about 9.90 with ammonia water. At the same time, NH4Cl was used to appropriately adjust the NH4 + The molar concentration of the substance was adjusted to the original concentration by using CuSO4·H2O. 2+ The mass concentration was returned to the original concentration, and the second experiment was carried out under the same current density, solid-liquid ratio and electrolysis time, and the process was repeated 7 times.

[0022] (2) After all the cycle experiments were completed, the cathode products, anode slag and electrolyte were collected, digested and tested for ICP, and the copper recovery rate of the waste mobile phone circuit boards, current efficiency, and cathode product copper purity were calculated. The results are shown in the following table.

[0023]

[0024] Example 2

[0025] In this embodiment, the metal copper in the waste mobile phone circuit board is recycled by alkaline slurry electrolyte. The process is as follows: Figure 1 shown.

[0026] (1) For the first electrolysis, prepare 200 mL of electrolyte, including 0.5 mol / L NaCl, 0.5 mol / L NH4Cl, 4 mol / L NH3·H2O, and 20 g / L Cu 2+ (CuSO4·5H2O). Add 6g WPCB-MPs powder into the anode chamber, stir, 20mA / cm 2 Electrolysis was carried out for 4 hours. After the electrolysis, the copper foil was collected from the cathode chamber, rinsed repeatedly with ultrapure water to wash away the copper-ammine complex on the surface of the copper foil, and then dried at 60°C to constant weight. The remaining slurry was filtered with a circulating water vacuum pump. The anode slag and the electrolyte were separated, where the anode slag was dried to constant weight at 60°C, and the separated electrolyte was used for the second cycle. During the second electrolysis, the remaining electrolyte after the first electrolysis was used, and the pH value of the electrolyte was adjusted to 9.90-10.0 with ammonia water, and the NH4Cl of the electrolyte was adjusted with NH4+ The concentration is 40-42g / L, and CuSO4·H2O is used to adjust the Cu 2+ The mass concentration is 20g / L. Preliminary experiments have shown that as the number of electrolyte cycles increases, metals other than copper will accumulate in the electrolyte, thereby reducing the copper recovery rate of WPCB-MPs and increasing the copper content in the anode slag. Therefore, the reaction time can be extended during the cycle to reduce the copper content in the anode residue. In addition, from the appearance of the cathode product, it can be seen that when the reaction time is extended, the appearance of the cathode copper foil obtained at the same current density will produce coking. Therefore, while extending the electrolysis time (4-6h), the current density (15-20mA / cm 2 ). Repeat the electrolyte 20 times using this method.

[0027] (2) After all the cycle experiments were completed, the cathode products, anode slag and electrolyte were collected, digested and tested for ICP, and the copper recovery rate of the waste mobile phone circuit boards, current efficiency, and cathode product copper purity were calculated. The results are as follows Figure 2 As shown. The experimental results of 19 times of electrolyte reuse show that copper is mainly distributed in the cathode product, and other metals are mainly distributed in the electrolyte and anode residue. With the increase in the number of cycles, the concentration of other metals in the electrolyte gradually increases, showing metal enrichment. Although the current efficiency fluctuates, it is basically higher than 90%. In addition, the recovery rate and purity of copper are basically unaffected. The copper recovery rate in waste mobile phone circuit boards is higher than 99%, the copper purity of the cathode product is higher than 99.9%, and all cathode copper foils are easy to fall off.

[0028] From the above examples, it can be seen that the present invention utilizes the circulation of electrolyte in ammonia-ammonium chloride alkaline slurry electrolysis to recover high-purity copper from WPCB-MPs, and deposits it on the cathode in the form of copper foil for recovery, wherein the copper recovery rate in waste mobile phone circuit boards is higher than 99%, the current efficiency is basically higher than 90%, and the cathode copper purity is higher than 99.9%. This method not only selectively realizes the deposition recovery of copper and reduces the generation of solid waste, but also reduces the use of chemical reagents in the recovery process, thereby saving costs and protecting the environment, providing a reference for the high-value resource recycling of waste circuit boards in alkaline slurry electrolysis.

[0029] Comparative Example 1

[0030] (1) For the first electrolysis, 200 mL of electrolyte was prepared, including 4 mol / L HCl, 100 g / L slurry concentration, and a current density of 80 mA / cm 2The electrolyte was electrolyzed for 4 hours and the pH value of the initial electrolyte was measured. Then, the remaining electrolyte obtained from the first electrolysis reaction was used as the electrolyte for the second electrolysis reaction. The pH was adjusted to the same as the first with HCl solution. The second experiment was carried out at the same current density, slurry concentration and reaction time. This method was repeated 14 times.

[0031] (2) After the reaction is completed, the cathode product, cation slag and electrolyte are collected in turn, digested and tested for ICP, and the copper recovery rate of the waste mobile phone circuit board, current efficiency, and cathode product copper purity are calculated. The results are as follows: Figure 3 As shown. After one slurry electrolysis reaction, the purity of the cathode copper powder was 90.23%, the current efficiency was 41.08%, and the recovery rate was 44.38%. With the recycling of the electrolyte, the changes of the three showed a fluctuating state. The copper powder recovery rate reached 71.58% after the second cycle, which was much higher than the recovery rate of a single electrolysis reaction. The highest copper powder recovery rate was obtained after the ninth cycle, which was 75.93%. Generally speaking, the recycling of the electrolyte has an adverse effect on the purity of the copper powder, because the continuous accumulation of metals in the electrolyte will lead to a higher content of impurities deposited at the cathode.

[0032] Through comparative experiments, it can be seen that ammonia-ammonium chloride alkaline slurry electrolysis can recover high-purity cathode copper foil from waste mobile phone circuit boards, and the recovery rate is high (basically greater than 99%), and the current efficiency (basically higher than 90%) is also much higher than the comparative experiment. Therefore, the use of the present invention not only selectively realizes the deposition recovery of copper and reduces the generation of solid waste, but also reduces the use of chemical reagents in the recovery process, thereby saving costs and protecting the environment, providing a reference for the high-value resource recycling of waste circuit boards by alkaline slurry electrolysis.

Claims

1. A method for recycling alkaline slurry electrolyte, It is characterized in that At least the following steps are included: S 1 , prepare an alkaline slurry electrolyte containing a certain concentration, add WPCB-MPs powder, and perform the first electrolysis at a certain current density; S 2 After the first electrolysis, the electrolyte was filtered and the separated electrolyte was adjusted to the following parameters before continuing the cyclic electrolysis: the pH of the electrolyte was adjusted to 9.80-10.0 with ammonia water, and the electrolyte was adjusted to 10.0 with NH 4 Cl regulates NH 4 + The molar concentration was 40-42 g / L using CuSO 4 ∙H 2 O regulates the Cu content in electrolyte 2+ The concentration is 20 g / L.

2. The method according to claim 1, It is characterized in that The alkaline slurry electrolyte includes 0.5 mol / L NaCl, 0.5 mol / L NH 4 Cl, 4 mol / L NH 3 ∙H 2 O, 20 g / L Cu 2+ .

3. The method according to claim 1, It is characterized in that WPCB-MPs powder is obtained by manually disassembling waste mobile phone circuit boards to remove components, then crushing them with a cutting crusher and passing them through a 40-mesh sieve.

4. The method according to claim 1, It is characterized in that The current density is 15-20 mA / cm 2 , preferably 20 mA / cm 2 ; The electrolysis time is 4-6 h, preferably 4 h.

5. The method according to claim 1, It is characterized in that The solid-liquid ratio during electrolysis was 30 g / L.