Process for simultaneously improving edge tearing and pinhole of ultra-thin copper foil
By adjusting the concentration of copper sulfate electrolyte and additives during the copper foil production process, the tensile strength and coil length of extremely thin copper foil are improved, tear and pinhole problems are solved, production costs are reduced, and lithium batteries are increased. performance.
Patent Information
- Application Number
- CN202410993053.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Extremely thin copper foils are prone to tear and pinholes during the production process, resulting in insufficient rolling meters and an increase in production costs, affecting the capacity and cycle life of lithium batteries.
By placing a copper sulfate electrolyte, adding a combination additive with inhibitor, brightener and leveling agent, electroplating is carried out under specific conditions, the concentration of the combined additive is adjusted to increase the tensile strength of the copper foil at room temperature and reduce the pinhole waste rice number.
The roll length and rolling number of 4.5μm extremely thin copper foil is significantly improved, which reduces production costs, improves production stability, reduces pinhole problems, and extends the service life of the battery.
Smart Images

Figure CN118932434A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electrolytic copper foil, in particular to a process for simultaneously improving edge tearing and pinholes in ultra-thin copper foil. Background Art
[0002] Copper foil is a cathodic electrolytic material. It is deposited on the substrate of the circuit board to form a thin, continuous metal foil. It is mainly used as a conductor for PCB (printed circuit board). Copper foil is mainly made of copper and a certain proportion of other metals. Common copper foils are 90% and 88%, that is, the copper content is 90% and 88% respectively. Copper foil has high conductivity, high thermal conductivity, and low surface oxygen characteristics. It can be attached to various substrates, such as metals, insulating materials, etc., and has a wide temperature range. Copper foil is widely used in electronics, electrical, construction, communications, printing and other fields, especially in electromagnetic shielding and antistatic performance. It is made by electrolysis under the action of direct current, and copper raw materials are made into copper sulfate solution and then electrodeposited. The production cost and technical threshold are low, and the application scale is large. It is mainly used in the production of lithium-ion batteries and printed circuit boards (PCBs). It is made by repeatedly rolling copper raw materials through physical means. The production cost is high and the technical threshold is high, but it has excellent mechanical properties such as high strength, high bendability, ductility, and better surface gloss. It is mainly used for flexible copper-clad laminates, electronic circuit boards, etc. A metal conductive layer is first made by vacuum sputtering on the surface of plastic films such as PET, PP, PI, and then the copper layer is thickened to 1 micron or more by water medium electroplating. The weight is relatively light compared to electrolytic copper foil, which can improve battery energy density, improve battery safety and reduce material costs. With the rapid development of the electronic information industry, the demand for copper foil continues to grow. In particular, high-performance electronic-grade copper foil, such as electrolytic copper foil and rolled copper foil, is increasingly in demand in the market. The continued growth in demand for copper foil in the domestic and foreign markets has promoted the rapid development of the copper foil industry. As an important cathodic electrolytic material, copper foil is widely used in electronics, electrical, construction, communications and other fields. With the continuous advancement of science and technology and the continuous growth of market demand, the copper foil industry will continue to maintain a rapid development trend.
[0003] Copper foil is a key component of lithium battery positive electrode materials, and its performance has an important impact on the performance of the entire lithium battery. At present, the thickness of the copper foil mainly used in the market is generally between 6-10 microns, but as the market's requirements for lithium battery performance and cost continue to increase, lithium battery manufacturers need to further reduce the thickness of copper foil in order to improve the energy density and power density of lithium batteries, reduce the weight of batteries, and reduce manufacturing costs.
[0004] At present, there are few copper foil factories that can stably produce 10,000-meter-level 4.5μm copper foil. The main problems in the production process are:
[0005] 1. The thickness of 4.5μm copper foil is extremely thin. The edge of the copper foil is easily torn during the production and reeling process, resulting in insufficient reeling of 4.5μm copper foil and inability to produce continuously, which greatly increases the production cost caused by reeling and reeling.
[0006] 2. The thinner the copper foil, the more likely it is to have pinholes during the production process. Copper foil with pinholes will have the risk of copper exposure during the coating process, thus affecting the capacity and cycle life of the battery;
[0007] In view of the above problems, a process for simultaneously improving the edge tearing and pinholes of ultra-thin copper foil is provided. Summary of the invention
[0008] The purpose of the present invention is to provide a process for simultaneously improving the tearing edge and pinholes of ultra-thin copper foil, so as to solve the problems raised in the above background technology. To achieve the above purpose, the present invention provides the following technical solution: A process for simultaneously improving the tearing edge and pinholes of ultra-thin copper foil, comprising the following steps:
[0009] Step 1, preparing a copper sulfate electrolyte by using sulfuric acid, copper and chloride ions;
[0010] Step 2, maintaining the electrolyte temperature within an appropriate range;
[0011] Step 3, adding a combination additive of inhibitor, brightener and leveler;
[0012] Step 4, in a foil production machine using an iridium-plated titanium anode plate as an anode and a titanium roller as a cathode;
[0013] Step 5, under the action of a DC power supply, electroplating a 4.5 μm ultra-thin copper foil on a cathode roller at a line speed of 11.252 m / min;
[0014] Step six, by adjusting the combined additives to a suitable concentration, the room temperature tensile strength of the copper foil is stabilized at 630MPa-670MPa, so that the roll length of the 4.5μm ultra-thin copper foil is increased and the number of pinholes in the copper foil is reduced.
[0015] Preferably, the concentration of the sulfuric acid is 90-120 g / L.
[0016] Preferably, in step 2, the electrolyte temperature is 50-55°C.
[0017] Preferably, the inhibitor comprises one or more of the group consisting of hydroxypropyl cellulose, hydroxyethyl cellulose, polyethylene glycol, and polypropylene glycol, preferably hydroxyethyl cellulose and polyethylene glycol.
[0018] Preferably, the brightener comprises one or more of sodium 3-mercapto-1-propane sulfonate, sodium polydisulfide propane sulfonate, sodium polydisulfide diethane sulfonate, o-benzoyl sulfonimide, sodium N,N-dimethyl disulfide propane sulfonate, and saccharin, preferably sodium polydisulfide propane sulfonate and o-benzoyl sulfonimide.
[0019] Preferably, the leveling agent comprises one or more of collagen peptides, gelatin, and collagen groups, preferably collagen peptides.
[0020] Preferably, in step five, the DC power supply current is 35000A.
[0021] Preferably, the concentration of the combined additive in step three is 0.1-20 mg / L.
[0022] Preferably, the copper concentration is 80-95 g / l.
[0023] Preferably, the chloride ion concentration is 10-20 mg / L.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] In this case, by adjusting the combined additives to an appropriate concentration, the room-temperature tensile strength of the copper foil is stabilized at 630MPa-670MPa, so that the roll length of the 4.5μm ultra-thin copper foil is increased, and the number of pinhole direct waste meters of the copper foil is reduced. The winding length of the 4.5μm ultra-thin copper foil can be increased from 10,000m to a maximum of 59,866m, which greatly reduces the production cost caused by winding and changing rolls, greatly improves the production stability of the 4.5μm ultra-thin copper foil, and solves the problem that the 4.5μm copper foil is extremely thin and the edges of the copper foil are easily torn during the production and winding process, resulting in insufficient winding length of the 4.5μm copper foil and inability to produce continuously, which greatly increases the production cost caused by winding and changing rolls, and the thinner the copper foil, the more likely it is to have pinholes in the production process. The copper foil with pinholes will have the risk of copper exposure during the coating process, thereby affecting the battery capacity and cycle life. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The present invention is a flowchart of a process for simultaneously improving edge tearing and pinholes in ultra-thin copper foil. DETAILED DESCRIPTION
[0027] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technical personnel in this field without creative work are within the scope of protection of the present invention.
[0028] See also Figure 1 The present invention provides a technical solution: a process for simultaneously improving the tearing edge and pinholes of ultra-thin copper foil, comprising the following steps:
[0029] Step 1, preparing a copper sulfate electrolyte by using sulfuric acid, copper and chloride ions;
[0030] Step 2, maintaining the electrolyte temperature within an appropriate range;
[0031] Step 3, adding a combination additive of inhibitor, brightener and leveler;
[0032] Step 4, in a foil production machine using an iridium-plated titanium anode plate as an anode and a titanium roller as a cathode;
[0033] Step 5, under the action of a DC power supply, electroplating a 4.5 μm ultra-thin copper foil on a cathode roller at a line speed of 11.252 m / min;
[0034] Step six, by adjusting the combined additives to a suitable concentration, the room temperature tensile strength of the copper foil is stabilized at 630MPa-670MPa, so that the roll length of the 4.5μm ultra-thin copper foil is increased and the number of pinholes in the copper foil is reduced.
[0035] In this embodiment, the concentration of sulfuric acid is 90-120 g / L.
[0036] In this embodiment, the electrolyte temperature in step 2 is 50-55°C.
[0037] In this embodiment, the inhibitor comprises one or more of the group consisting of hydroxypropyl cellulose, hydroxyethyl cellulose, polyethylene glycol, and polypropylene glycol, preferably hydroxyethyl cellulose and polyethylene glycol. Hydroxypropyl cellulose is insoluble in benzene and ether at room temperature, but soluble in polar organic solvents such as water, methanol, ethanol, and isopropanol. It has good thermoplasticity, film-forming properties, adhesion, and antibacterial properties, is chemically inert, and is difficult to react chemically with other substances. It is mainly used in the pharmaceutical industry as a binder for tablets, granules, and fine particles, as well as a disintegrant for tablets, and is also used in daily Chemical industry, such as the manufacture of creams, shampoos, lotions and other cosmetics. Hydroxyethyl cellulose is a non-ionic cellulose derivative that is soluble in organic solvents and water, but insoluble in alcohols and esters. It has a high viscosity, usually between 2000-10000cp, and has good acid and alkali resistance and high temperature resistance. It is widely used in construction, oil fields, medicine and other fields as a thickener, fluid loss reducer, clay stabilizer, etc. It is also used as a dispersant in coatings, paints, papermaking and other industries. Polyethylene glycol is a high molecular polymer with a chemical formula of HO(CH 2 CH 2O)H, soluble in water, ethanol and many other organic solvents, has excellent lubricity, moisturizing, dispersibility and adhesion, is non-toxic and non-irritating, and is used in cosmetics, pharmaceuticals, chemical fiber, rubber, plastics, papermaking, paints, electroplating, pesticides, metal processing and food processing industries. It is widely used in a variety of pharmaceutical preparations, such as injections, topical preparations, ophthalmic preparations, oral and rectal preparations. Propylene glycol is a compound with a similar structure to polyethylene glycol, but the carbon chain on the main chain is longer. It is usually soluble in a variety of organic solvents, but the specific solubility may vary depending on the molecular weight. It has low volatility and good stability and is mainly used in industrial fields, such as as a solvent, plasticizer, lubricant, etc. It also has certain applications in the cosmetics and pharmaceutical industries, but relatively few.
[0038] In this embodiment, the brightener comprises one or more of sodium 3-mercapto-1-propane sulfonate, sodium polydisulfide propane sulfonate, sodium polydisulfide diethane sulfonate, o-benzoyl sulfonimide, sodium N,N-dimethyl disulfide propane sulfonate, and saccharin, preferably sodium polydisulfide propane sulfonate and o-benzoyl sulfonimide. Sodium 3-mercapto-1-propane sulfonate is used as a brightener for acid copper plating to improve the decorativeness and functionality of the coating. It is generally used in combination with polyethers and non-ionic surfactants to improve the brightness and ductility of the coating. If polyamines, dyes and other sulfur-containing compounds are added, the effect is better. Polydisulfide propane sulfonate Sodium sulfate, white or light yellow powder, easy to absorb moisture, strong water solubility, slightly soluble in alcohols, important electrolyte additive, used in acid copper plating brightener, can obtain decorative and functional coatings (such as printed circuit boards), can be used in combination with non-ionic surfactants, polyamines and other thiol compounds in typical copper plating formulas, and can also be used in combination with dyes to enhance the effect, o-benzoylsulfonyl imide, white crystalline powder, mainly used as a sweetener, sweetness is 300 to 500 times that of sucrose, used in food industry, toothpaste, cigarettes and cosmetics, saccharin is mainly used as a sweetener, widely used in food industry, toothpaste, cigarettes and cosmetics.
[0039] In this embodiment, the leveling agent includes one or more of collagen peptides, gelatin, and collagen group, preferably collagen peptides. Collagen peptides are an extracellular protein, a small molecule peptide composed of two or more amino acids. It is a small molecule peptide formed after collagen is treated with artificial protease. It has a small molecular weight, usually between 1000-3000 Daltons, and is easily absorbed by the human body. Collagen peptides form a fine elastic network in the skin, which can lock in moisture, support the skin, reduce wrinkles and sagging, and help maintain the elasticity and luster of hair. Gelatin is a macromolecular hydrophilic colloid, a product of partial hydrolysis of collagen, with a certain molecular weight distribution, which varies due to different process conditions and affects the physical and chemical properties of gelatin. Gelatin is colorless to light yellow, in powder, flake or block form, shiny, odorless and tasteless. It can be divided into photographic gelatin, edible gelatin and industrial gelatin according to its performance and use. Photographic gelatin is mainly used in the photography industry, and edible gelatin is widely used in In the food industry, such as candy, jelly, dairy products, etc., industrial gelatin is used to make adhesives, coatings, etc. Gelatin is insoluble in water, but when soaked in water, it can absorb 5 to 10 times the water and swell and soften. When heated, it dissolves into a colloid and forms a gel after cooling. It has a certain viscosity and elasticity. Collagen is a biological polymer and the main component of animal connective tissue. It is also the most abundant and widely distributed functional protein in mammals. It accounts for 25%-30% of the total protein and plays the role of binding tissue in animal cells. There are many types of collagen, the most common of which are type I, type II, type III, type V and type VI. It is mainly found in animal skin, bone, cartilage, tendon, ligament and other tissues to maintain skin elasticity: Collagen is the main component of skin elastic fibers, which helps to maintain skin moisture and elasticity. It is widely used in food, medicine, tissue engineering, cosmetics and other fields. In the medical field, collagen can be used to make medical supplies such as collagen sponges, collagen membranes and artificial skin.
[0040] In this embodiment, the DC power supply current in step five is 35000A. The DC power supply is a power supply device that can stably output DC power. Its characteristic is that the current flow direction remains unchanged from the positive pole to the negative pole. The DC power supply is a device that maintains a constant voltage and current in the circuit, such as a dry cell, a storage battery, a DC generator, etc. It converts other forms of energy into electrical energy to supply the circuit to maintain a constant flow of current. The DC power supply has positive and negative electrodes. The positive electrode has a high potential and the negative electrode has a low potential. When the two electrodes are connected to the circuit, a constant potential difference can be maintained between the two ends of the circuit, thereby forming a current from the positive pole to the negative pole in the external circuit. The DC power supply is an energy conversion device. The basic principle is similar to the process of a water pump maintaining a water level difference to form a constant water flow. The working principle of the DC power supply is based on the rectification process, that is, converting the input AC signal into a pulse signal with only a positive half cycle (or a negative half cycle), and then converting these pulse signals into a stable DC signal through a filtering circuit. The rectification process is mainly composed of a diode, a transformer and a filter capacitor. The voltage regulation coefficient refers to the load current and ambient temperature when the load current and ambient temperature remain unchanged. , the relative change of input voltage causes the relative change of output voltage. Voltage regulation refers to the relative change of output voltage when the relative change of input voltage is ±10%. Both parameters describe the influence of input voltage change on output voltage. Output resistance is the same as the output resistance of the amplifier. Its value is the absolute value of the ratio of output voltage change to output current change when the input voltage remains unchanged. Current regulation refers to the relative change of output voltage when the output current changes from 0 to the maximum value. Both parameters describe the influence of load current change on output voltage. The AC voltage component superimposed on the output voltage is generally in the millivolt range when observed with an oscilloscope. Its effective value can also be measured with an AC millivoltmeter. However, because the ripple is not a sine wave, there is a certain error. According to different application scenarios and requirements, there are many types of DC power supplies, such as linear DC regulated power supplies and switching DC power supplies. Linear DC regulated power supplies are mainly used for electrical and electrical instrument detection or power supply. They have the characteristics of high output accuracy, strong anti-interference ability and small ripple. Switching DC power supplies are mainly used for industrial equipment. They have the characteristics of high power and small size.
[0041] In this embodiment, the concentration of the combined additive in step 3 is 0.1-20 mg / L.
[0042] In this embodiment, the copper concentration is 80-95 g / l.
[0043] In this embodiment, the chloride ion concentration is 10-20 mg / L. - ) is a chlorine-1 ion widely found in nature, with a series of important physiological and chemical properties. Chloride ions often participate as ligands or reactants in chemical reactions, such as with silver ions (Ag +) reacts to generate insoluble silver chloride (AgCl) precipitate, which is one of the common methods for detecting chloride ions. The existence state of chloride ions in solution is affected by the pH value of the solution. Changes in pH value may affect the activity coefficient and solubility of chloride ions. In the chemical industry, the presence of chloride ions may corrode equipment, especially long-term high chloride ion content in circulating water will cause serious corrosion and cracking to equipment such as austenitic stainless steel. The catalytic effect of chloride ions may also cause stress corrosion cracking of stainless steel equipment. Therefore, in practical applications, it is necessary to strictly control the chloride ion content and take corresponding protective measures. There are many methods for detecting chloride ions, among which acid silver titration is a commonly used method. This method adds a certain amount of silver nitrate standard solution to a slightly acidic solution to make chloride ions become silver chloride precipitate, and then determines the chloride ion content by titrating excess silver nitrate. In addition, there are other detection methods such as potentiometric titration and ion chromatography.
[0044] Example 1
[0045] A copper sulfate electrolyte is maintained at a constant temperature of 50-55°C, wherein the sulfuric acid concentration is 90-120 g / L, the copper concentration is 80-95 g / L, and the chloride ion concentration is 10-20 ppm;
[0046] The concentration of hydroxyethyl cellulose is 15 mg / L, the concentration of sodium polydisulfide propane sulfonate is 10 mg / L, the concentration of collagen peptide is 4 mg / L, the concentration of polyethylene glycol is 5 mg / L, and the concentration of o-toluene sulfonimide is 0.5 mg / L. The continuous winding length of the 4.5 μm ultra-thin copper foil produced in this embodiment is 39853 m, the tensile strength at room temperature is 675.57 MPa, and the pinhole straight waste length is 108 m.
[0047] Example 2
[0048] A copper sulfate electrolyte is maintained at a constant temperature of 50-55°C, wherein the sulfuric acid concentration is 90-120 g / L, the copper concentration is 80-95 g / L, and the chloride ion concentration is 10-20 ppm;
[0049] The concentration of hydroxyethyl cellulose is 7 mg / L, the concentration of sodium polydisulfide propane sulfonate is 5 mg / L, the concentration of collagen peptide is 4 mg / L, the concentration of polyethylene glycol is 4 mg / L, and the concentration of o-toluene sulfonyl imide is 0.6 mg / L. The continuous winding length of the 4.5 μm ultra-thin copper foil produced in this embodiment is 59866 m, the tensile strength at room temperature is 656.88 MPa, and the pinhole straight waste length is 19 m.
[0050] Example 3
[0051] A copper sulfate electrolyte is maintained at a constant temperature of 50-55°C, wherein the sulfuric acid concentration is 90-120 g / L, the copper concentration is 80-95 g / L, and the chloride ion concentration is 10-20 ppm;
[0052] The concentration of hydroxyethyl cellulose is 3 mg / L, the concentration of sodium polydisulfide propane sulfonate is 3 mg / L, the concentration of collagen peptide is 7 mg / L, the concentration of polyethylene glycol is 3 mg / L, and the concentration of o-toluene sulfonimide is 0.5 mg / L. The continuous winding length of the 4.5 μm ultra-thin copper foil produced in this embodiment is 45889 m, the tensile strength at room temperature is 648.66 MPa, and the pinhole straight waste length is 73 m.
[0053] Example 4
[0054] A copper sulfate electrolyte is maintained at a constant temperature of 50-55°C, wherein the sulfuric acid concentration is 90-120 g / L, the copper concentration is 80-95 g / L, and the chloride ion concentration is 10-20 ppm;
[0055] The concentration of hydroxyethyl cellulose is 6 mg / L, the concentration of sodium polydisulfide propane sulfonate is 5.5 mg / L, the concentration of collagen peptide is 12 mg / L, the concentration of polyethylene glycol is 7 mg / L, and the concentration of o-toluene sulfonyl imide is 1 mg / L. The continuous winding length of the 4.5 μm ultra-thin copper foil produced in this embodiment is 36871 m, the tensile strength at room temperature is 635.57 MPa, and the pinhole straight waste length is 134 m.
[0056] Control group 1
[0057] A copper sulfate electrolyte is maintained at a constant temperature of 50-55°C, wherein the sulfuric acid concentration is 90-120 g / L, the copper concentration is 80-95 g / L, and the chloride ion concentration is 10-20 ppm;
[0058] The concentration of hydroxyethyl cellulose is 15 mg / L, the concentration of sodium polydisulfide propane sulfonate is 10 mg / L, and the concentration of collagen peptide is 4 mg / L. The continuous winding length of the 4.5 μm ultra-thin copper foil produced in this embodiment is 11721 m, the tensile strength at room temperature is 586.33 MPa, and the pinhole straight waste length is 235 m.
[0059] Control group 2
[0060] A copper sulfate electrolyte is maintained at a constant temperature of 50-55°C, wherein the sulfuric acid concentration is 90-120 g / L, the copper concentration is 80-95 g / L, and the chloride ion concentration is 10-20 ppm;
[0061] The concentration of hydroxyethyl cellulose is 4 mg / L, the concentration of sodium polydisulfide propane sulfonate is 4.4 mg / L, and the concentration of collagen peptide is 9 mg / L. The continuous winding length of the 4.5 μm ultra-thin copper foil produced in this embodiment is 10745 m, the tensile strength at room temperature is 612.79 MPa, and the pinhole straight waste length is 398 m.
[0062] In this case, by adjusting the combined additives to a suitable concentration, the room temperature tensile strength of the copper foil is stabilized at 630MPa-670MPa, so that the roll length of the 4.5μm ultra-thin copper foil is increased, and the number of pinhole direct waste meters of the copper foil is reduced. The winding length of the 4.5μm ultra-thin copper foil can be increased from 10,000m to a maximum of 59,866m, which greatly reduces the production cost caused by winding and changing rolls, greatly improves the production stability of the 4.5μm ultra-thin copper foil, and solves the problem that the 4.5μm copper foil is extremely thin and the edges of the copper foil are easily torn during the production and winding process, resulting in insufficient winding length of the 4.5μm copper foil and inability to produce continuously, which greatly increases the production cost caused by rolling and changing rolls, and the thinner the copper foil, the more likely it is to have pinholes in the production process. The copper foil with pinholes will have the risk of copper exposure during the coating process, thereby affecting the battery capacity and cycle life.
[0063] The above shows and describes the basic principles, main features and advantages of the present invention. Technical personnel in this industry should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only preferred examples of the present invention and are not used to limit the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A process for simultaneously improving the tearing and pinholes of ultra-thin copper foil. It is characterized in that The steps include: Step 1, preparing a copper sulfate electrolyte by using sulfuric acid, copper and chloride ions; Step 2, maintaining the electrolyte temperature within an appropriate range; Step 3, adding a combination additive of inhibitor, brightener and leveler; Step 4, in a foil production machine using an iridium-plated titanium anode plate as an anode and a titanium roller as a cathode; Step 5, under the action of a DC power supply, electroplating a 4.5 μm ultra-thin copper foil on a cathode roller at a line speed of 11.252 m / min; Step six, by adjusting the combined additives to a suitable concentration, the room temperature tensile strength of the copper foil is stabilized at 630MPa-670MPa, so that the roll length of the 4.5μm ultra-thin copper foil is increased and the number of pinholes in the copper foil is reduced.
2. A process for simultaneously improving edge tearing and pinholes in ultra-thin copper foil according to claim 1, Features: The concentration of the sulfuric acid is 90-120 g / L.
3. A process for simultaneously improving edge tearing and pinholes in ultra-thin copper foil according to claim 1, Features: In step 2, the electrolyte temperature is 50-55°C.
4. A process for simultaneously improving edge tearing and pinholes in ultra-thin copper foil according to claim 1, Features: The inhibitor comprises one or more of the group consisting of hydroxypropyl cellulose, hydroxyethyl cellulose, polyethylene glycol, and polypropylene glycol, preferably hydroxyethyl cellulose and polyethylene glycol.
5. A process for simultaneously improving edge tearing and pinholes in ultra-thin copper foil according to claim 1, Features: The brightener comprises one or more of sodium 3-mercapto-1-propane sulfonate, sodium polydipropane disulfide sulfonate, sodium polydiethane disulfide sulfonate, o-benzoyl sulfonimide, sodium N,N-dimethyl dithiocarboxamide propane sulfonate, and saccharin, preferably sodium polydipropane disulfide sulfonate and o-benzoyl sulfonimide.
6. A process for simultaneously improving edge tearing and pinholes in ultra-thin copper foil according to claim 1, Features: The leveling agent comprises one or more of collagen peptide, gelatin and collagen, preferably collagen peptide.
7. The process for simultaneously improving edge tearing and pinholes in ultra-thin copper foil according to claim 1, Features: In step 5, the DC power supply current is 35000A.
8. The process for simultaneously improving edge tearing and pinholes in ultra-thin copper foil according to claim 1, Features: The concentration of the combined additive in step three is 0.1-20 mg / L.
9. The process for simultaneously improving edge tearing and pinholes of ultra-thin copper foil according to claim 1, Features: The copper concentration is 80-95 g / l.
10. A process for simultaneously improving edge tearing and pinholes in ultra-thin copper foil according to claim 1, Features: The chloride ion concentration is 10-20 mg / L.
Citation Information
Cited By
Manufacturing methods for controlling the number of pinholes in electrolytic copper foil, copper foil, and applications of copper foil