Electrolytic nitrogen removal method for high-temperature alloy return scraps

By electrolyzing the nickel-based high-temperature alloy return material, and using hydrochloric acid or sulfuric acid solution to remove the nitride layer on its surface, the problem of nitrogen layer in the high-temperature alloy return material affecting the purity of smelting, and effectively reducing nitrogen content and improving resource utilization rate effect.

CN118932470APending Publication Date: 2024-11-12JIANGSU LONGXIANG SPECIAL MATERIALS TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411158506.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The surface of the high-temperature alloy return material contains a nitrogen layer, which affects the purity of the smelted master alloy. It is difficult for the prior art to effectively reduce the nitrogen content.

Method used

The nickel-based high-temperature alloy return material was treated by electrolysis, and electrolyzed with 20%-30% hydrochloric acid or sulfuric acid solution was used to control the voltage and current, and then rinsed with clean water and dried in an oven to remove the nitride layer.

Benefits of technology

Effectively reduce the nitrogen content of the return material, improve the purity of the smelted master alloy, reduce resource waste, reduce enterprise costs, and improve the utilization rate of the return material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005005761730000041
    Figure BDA0005005761730000041
Patent Text Reader

Abstract

The invention relates to an electrolytic nitrogen removal method for nickel-based high-temperature alloy return scraps. The method comprises the following steps that the nickel-based high-temperature alloy return scraps are cut into nickel-based high-temperature alloy blocks; the nickel-based high-temperature alloy block is put into an electrolytic tank of electrolysis equipment, a hydrochloric acid solution and a sulfuric acid solution are adopted as electrolyte, electrodes are connected, and a power source is started for electrolysis treatment; and after electrolysis is completed, the nickel-based high-temperature alloy block is washed with clear water, after washing is completed, the nickel-based high-temperature alloy block is put into a drying oven to be dried, and finally the nickel-based high-temperature alloy block with the nitride layer removed is obtained. The method is simple in operation step and convenient to operate, the nitrogen content of the surface of the high-temperature alloy return scrap can be effectively reduced, the burden of a subsequent smelting process is relieved, meanwhile, resource waste is greatly reduced through treatment and reutilization of the return scrap, and the cost of an enterprise is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of high-temperature alloy return material processing, and in particular relates to a method for electrolytic denitrification of high-temperature alloy return materials. Background Art

[0002] In the production process of high-temperature alloys, a large number of material heads, risers, runners, and scrapped parts are generated, so the utilization rate of high-temperature alloys is low. In order to reduce the cost and energy consumption of high-temperature alloys, reduce the loss of precious metals, protect the environment and recycle resources, returned materials begin to be used in the smelting process. In order to ensure the purity of the smelting, the O and N content of the returned materials needs to be strictly controlled.

[0003] There is a nitrogen-containing layer on the surface of the high-temperature alloy return material. If the nitrogen-containing layer is not cleaned, it will have a great impact on the purity of the smelted master alloy. Therefore, how to effectively reduce the nitrogen content in the return material becomes a top priority. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for electrolytic denitrification of high-temperature alloy return material which can effectively reduce the nitrogen content on the surface.

[0005] According to the technical solution provided by the present invention, the method for electrolytic denitrification of the nickel-based high-temperature alloy return material comprises the following steps:

[0006] S1. Cutting the nickel-based high-temperature alloy return material into nickel-based high-temperature alloy blocks;

[0007] S2, placing the nickel-based high-temperature alloy block into the electrolytic cell of the electrolytic equipment, using a hydrochloric acid solution with a mass percentage concentration of 20%-30% or a sulfuric acid solution with a mass percentage concentration of 20%-30%, connecting the electrodes, starting the power supply for electrolysis, the power supply voltage of the electrolytic cell is 220V, the current is controlled at 3-5mA, and the electrolysis time is controlled at 30-50 minutes;

[0008] S3. After the electrolysis is completed, the nickel-based high-temperature alloy block is rinsed with clean water. After the rinsing is completed, the nickel-based high-temperature alloy block is placed in an oven for drying, the temperature is controlled at 100-120° C., and the time is controlled at 10-12 hours, and finally a nickel-based high-temperature alloy block with the nitride layer removed is obtained.

[0009] Preferably, the dimension of any side of the nickel-based high-temperature alloy block is less than or equal to 300 mm.

[0010] The method of the present invention has simple operating steps and is easy to operate. It can effectively reduce the nitrogen content on the surface of high-temperature alloy return materials, thereby reducing the burden on subsequent smelting processes. At the same time, the processing and reuse of return materials greatly reduces resource waste and reduces enterprise costs. DETAILED DESCRIPTION

[0011] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution of the present invention will be clearly and completely described in combination with the specific embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.

[0012] Example 1

[0013] A method for electrolytic denitrification of a nickel-based high-temperature alloy return material with a grade of K452. The mass percentage of inclusions in the nickel-based high-temperature alloy return material is 2%, the N content is 60 ppm, and the area proportion of slag is 5%. The denitrification method comprises the following steps:

[0014] S1. Cut the nickel-based high-temperature alloy return material into cubic nickel-based high-temperature alloy blocks, and the size of any side of the nickel-based high-temperature alloy block is equal to 200 mm.

[0015] S2, placing the nickel-based high-temperature alloy block into the electrolytic cell of the electrolytic equipment, using a hydrochloric acid solution with a mass percentage concentration of 20% as the electrolyte, connecting the electrodes, starting the power supply for electrolysis, the power supply voltage of the electrolytic cell is 220V, the current is controlled at 3mA, and the electrolysis time is controlled at 30 minutes;

[0016] S3. After the electrolysis is completed, the nickel-based high-temperature alloy block is rinsed with clean water. After the rinsing is completed, the nickel-based high-temperature alloy block is placed in an oven for drying, the temperature is controlled at 100° C., and the time is controlled at 10 hours, and finally a nickel-based high-temperature alloy block with the nitride layer removed is obtained.

[0017] Example 2

[0018] A method for electrolytic denitrification of a nickel-based high-temperature alloy return material with a grade of K444, wherein the mass percentage of inclusions in the nickel-based high-temperature alloy return material is 3%, the N content is 70 ppm, and the area proportion of slag is 5%. The denitrification method comprises the following steps:

[0019] S1. Cut the nickel-based high-temperature alloy return material into cubic nickel-based high-temperature alloy blocks, and the size of any side of the nickel-based high-temperature alloy block is equal to 250 mm.

[0020] S2, placing the nickel-based high-temperature alloy block into the electrolytic cell of the electrolytic equipment, using a hydrochloric acid solution with a mass percentage concentration of 25% as the electrolyte, connecting the electrodes, starting the power supply for electrolysis, the power supply voltage of the electrolytic cell is 220V, the current is controlled at 4mA, and the electrolysis time is controlled at 40 minutes;

[0021] S3. After the electrolysis is completed, the nickel-based high-temperature alloy block is rinsed with clean water. After the rinsing is completed, the nickel-based high-temperature alloy block is placed in an oven for drying. The temperature is controlled at 110° C. and the time is controlled at 11 hours to finally obtain a nickel-based high-temperature alloy block with the nitride layer removed.

[0022] Example 3

[0023] A method for electrolytic denitrification of a nickel-based high-temperature alloy return material with a grade of K465. The mass percentage of inclusions in the nickel-based high-temperature alloy return material is 4%, the N content is 80 ppm, and the area proportion of slag is 5%. The denitrification method comprises the following steps:

[0024] S1. Cut the nickel-based high-temperature alloy return material into cubic nickel-based high-temperature alloy blocks, and the size of any side of the nickel-based high-temperature alloy block is equal to 300 mm.

[0025] S2, placing the nickel-based high-temperature alloy block into the electrolytic cell of the electrolytic equipment, using a hydrochloric acid solution with a mass percentage concentration of 30% as the electrolyte, connecting the electrodes, starting the power supply for electrolysis, the power supply voltage of the electrolytic cell is 220V, the current is controlled at 5mA, and the electrolysis time is controlled at 50 minutes;

[0026] S3. After the electrolysis is completed, the nickel-based high-temperature alloy block is rinsed with clean water. After the rinsing is completed, the nickel-based high-temperature alloy block is placed in an oven for drying. The temperature is controlled at 120° C. and the time is controlled at 12 hours to finally obtain a nickel-based high-temperature alloy block with the nitride layer removed.

[0027] Example 4

[0028] A method for electrolytic denitrification of a nickel-based high-temperature alloy return material with a grade of K452. The mass percentage of inclusions in the nickel-based high-temperature alloy return material is 3%, the N content is 65ppm, and the area proportion of slag is 5%. The denitrification method comprises the following steps:

[0029] S1. Cut the nickel-based high-temperature alloy return material into cubic nickel-based high-temperature alloy blocks, and the size of any side of the nickel-based high-temperature alloy block is equal to 200 mm.

[0030] S2, placing the nickel-based high-temperature alloy block into the electrolytic cell of the electrolytic equipment, using a sulfuric acid solution with a mass percentage concentration of 20% as the electrolyte, connecting the electrodes, starting the power supply for electrolysis, the power supply voltage of the electrolytic cell is 220V, the current is controlled at 3mA, and the electrolysis time is controlled at 30 minutes;

[0031] S3. After the electrolysis is completed, the nickel-based high-temperature alloy block is rinsed with clean water. After the rinsing is completed, the nickel-based high-temperature alloy block is placed in an oven for drying, the temperature is controlled at 100° C., and the time is controlled at 10 hours, and finally a nickel-based high-temperature alloy block with the nitride layer removed is obtained.

[0032] Example 5

[0033] A method for electrolytic denitrification of a nickel-based high-temperature alloy return material with a grade of K444. The mass percentage of inclusions in the nickel-based high-temperature alloy return material is 4%, the N content is 72ppm, and the area proportion of slag is 5%. The denitrification method comprises the following steps:

[0034] S1. Cut the nickel-based high-temperature alloy return material into cubic nickel-based high-temperature alloy blocks, and the size of any side of the nickel-based high-temperature alloy block is equal to 250 mm.

[0035] S2, placing the nickel-based high-temperature alloy block into the electrolytic cell of the electrolytic equipment, using a sulfuric acid solution with a mass percentage concentration of 25% as the electrolyte, connecting the electrodes, starting the power supply for electrolysis, the power supply voltage of the electrolytic cell is 220V, the current is controlled at 4mA, and the electrolysis time is controlled at 40 minutes;

[0036] S3. After the electrolysis is completed, the nickel-based high-temperature alloy block is rinsed with clean water. After the rinsing is completed, the nickel-based high-temperature alloy block is placed in an oven for drying. The temperature is controlled at 110° C. and the time is controlled at 11 hours to finally obtain a nickel-based high-temperature alloy block with the nitride layer removed.

[0037] Example 6

[0038] A method for electrolytic denitrification of a nickel-based high-temperature alloy return material with a grade of K465. The mass percentage of inclusions in the nickel-based high-temperature alloy return material is 5%, the N content is 77 ppm, and the area proportion of slag is 5%. The denitrification method comprises the following steps:

[0039] S1. Cut the nickel-based high-temperature alloy return material into cubic nickel-based high-temperature alloy blocks, and the size of any side of the nickel-based high-temperature alloy block is equal to 300 mm.

[0040] S2, placing the nickel-based high-temperature alloy block into the electrolytic cell of the electrolytic equipment, using a sulfuric acid solution with a mass percentage concentration of 30% as the electrolyte, connecting the electrodes, starting the power supply for electrolysis, the power supply voltage of the electrolytic cell is 220V, the current is controlled at 5mA, and the electrolysis time is controlled at 50 minutes;

[0041] S3. After the electrolysis is completed, the nickel-based high-temperature alloy block is rinsed with clean water. After the rinsing is completed, the nickel-based high-temperature alloy block is placed in an oven for drying. The temperature is controlled at 120° C. and the time is controlled at 12 hours to finally obtain a nickel-based high-temperature alloy block with the nitride layer removed.

[0042] The performance test results of the nickel-based high-temperature alloy blocks obtained by electrolytic denitrification of Examples 1-6 are shown in Table 1.

[0043] Table 1

[0044]

[0045] As can be seen from Table 1, the inclusions, N content and slag content of the mother alloy after smelting of the nickel-based high-temperature alloy return material treated by the present invention can meet the technical requirements and are equivalent to the level of new materials, indicating that the present invention has a good treatment effect.

[0046] The method for electrolytic denitrification of nickel-based high-temperature alloy return material of the present invention has a clear process concept and simple and executable steps. The return material after electrolytic denitrification can remove a nitride layer, which significantly reduces the nitrogen content of the return material, thereby reducing the burden on subsequent smelting processes. At the same time, the processing and reuse of the return material greatly reduces resource waste, reduces the cost of the enterprise, and has high economic value.

[0047] The method for electrolytic denitrification of nickel-based high-temperature alloy return material of the present invention can effectively remove non-metallic slag inclusions, residual dust, rust, scale, coating, oil stains, water stains and other attachments on the surface of the block return material, can effectively control the depth of removal of the nitrogen-containing layer, greatly improve the scum level after remelting the block return material, improve the utilization rate of the return material, and ensure the purity of the master alloy smelting.

[0048] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. A method for electrolytic denitrification of nickel-based high-temperature alloy return material, characterized in that The nitrogen removal method comprises the following steps: S1. Cutting the nickel-based high-temperature alloy return material into nickel-based high-temperature alloy blocks; S2, placing the nickel-based high-temperature alloy block into the electrolytic cell of the electrolytic equipment, using a hydrochloric acid solution with a mass percentage concentration of 20%-30% or a sulfuric acid solution with a mass percentage concentration of 20%-30%, connecting the electrodes, starting the power supply for electrolysis, the power supply voltage of the electrolytic cell is 220V, the current is controlled at 3-5mA, and the electrolysis time is controlled at 30-50 minutes; S3. After the electrolysis is completed, the nickel-based high-temperature alloy block is rinsed with clean water. After the rinsing is completed, the nickel-based high-temperature alloy block is placed in an oven for drying, the temperature is controlled at 100-120° C., and the time is controlled at 10-12 hours, and finally a nickel-based high-temperature alloy block with the nitride layer removed is obtained.

2. The method for electrolytic denitrification of high temperature alloy return material according to claim 1, characterized in that: The dimension of any side of the nickel-based high-temperature alloy block is less than or equal to 300 mm.